Neil Sheward
Technical Services Manager
Fatigue Enhancement of Critical Components by
Controlled Shot-Peening & Laser-Peening
![Page 2: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/2.jpg)
![Page 3: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/3.jpg)
CW Flow Control MIC Material Treatments CW Motion Control
![Page 4: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/4.jpg)
MIC International Facilities
USA
Sweden
China
UK France
Spain
Germany
Italy Belgium
Canada
China
3 facilities
Europe
3 facilities
Singapore
1 facility
Austria
A Global Organisation
Over 60 Divisions in 11 Countries
![Page 5: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/5.jpg)
Metal Improvement Company UK Divisions
![Page 6: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/6.jpg)
Controlled Shot-Peening
Super-Finishing
Site Work
Laser-Peening
Peen Forming
Peenflex Protective Mouldings
![Page 7: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/7.jpg)
“Improving the fatigue life of critical components”
Aircraft superstructures
Aero engine components
Landing gear
Fasteners and fittings
![Page 8: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/8.jpg)
“When the work is too big for our site .... our site goes to the work” Aircraft superstructures
Vessels
Power stations
Industrial applications
![Page 9: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/9.jpg)
“CASE isotropic and vibratory polishing”
Gears
Shafts
Turbine blades
![Page 10: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/10.jpg)
“Using the latest technology to achieve very deep levels of residual stress”
Discs
Drums
Blisks
Turbine blades
![Page 11: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/11.jpg)
“Using Shot peening technology to provide form and fatigue strength”
Wing skins
Wing struts
Stringers
![Page 12: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/12.jpg)
“Design and manufacture of bespoke mouldings”
Peen masking
Damage protection
Work-holding
![Page 13: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/13.jpg)
The effects of peening have been long known
2700 BC Peening of
Gold Helmets and Weapons
1200 AD Peening of armour and
swords during crusades
1945 John Almen – Effects of Shot
Blasting on Mechanical Properties of Steel
1949 METAL IMPROVEMENT
COMPANY formed
![Page 14: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/14.jpg)
Shot peening is the bombardment of a metallic surface with spherical media
The primary benefit of Shot-Peening is an increased resistance to fatigue
![Page 15: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/15.jpg)
Progressive localised damage from cyclic loads of less than the material UTS
Crack initiation site
Slow crack growth
Sudden fracture
![Page 16: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/16.jpg)
Stage 1 HPT Disc Fatigue failure
The consequences of fatigue can
be catastrophic
![Page 17: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/17.jpg)
Cast steel shot
Cut wire shot
Glass bead
Ceramic bead
Media Impact Creates a Surface Dimple
Optimum peening conditions are achieved by selecting appropriate media and intensity
0-45deg
![Page 18: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/18.jpg)
SUB-SURFACE YIELDS
IMPACT
![Page 19: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/19.jpg)
COMPRESSION
IMPACT
Compressive forces attempt to restore the deformed layer to its original condition
![Page 20: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/20.jpg)
Stretched Surface is restrained by mass below
![Page 21: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/21.jpg)
![Page 22: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/22.jpg)
![Page 23: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/23.jpg)
![Page 24: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/24.jpg)
![Page 25: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/25.jpg)
![Page 26: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/26.jpg)
![Page 27: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/27.jpg)
![Page 28: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/28.jpg)
METAL FATIGUE CRACKS WILL ONLY OCCUR WHERE THE METAL IS IN TENSION
NEVER WHERE THE METAL IS IN COMPRESSION
TENSION
COMPRESSION
![Page 29: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/29.jpg)
Therefore by introducing a compressive stress to the area in tension.....
…..an increased resistance to metal fatigue is achieved
COMPRESSION
COMPRESSION
![Page 30: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/30.jpg)
METAL FATIGUE CRACKS WILL ONLY OCCUR WHERE
THE METAL IS IN TENSION
NEVER WHERE THE METAL IS IN COMPRESSION
COMPRESSION
COMPRESSION
![Page 31: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/31.jpg)
METAL FATIGUE CRACKS WILL ONLY OCCUR WHERE
THE METAL IS IN TENSION
NEVER WHERE THE METAL IS IN COMPRESSION
COMPRESSION
COMPRESSION
![Page 32: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/32.jpg)
METAL FATIGUE CRACKS WILL ONLY OCCUR WHERE
THE METAL IS IN TENSION
NEVER WHERE THE METAL IS IN COMPRESSION
COMPRESSION
COMPRESSION
![Page 33: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/33.jpg)
Sources of Stress
Vibration Pressure Thermal Bolting Dead Load
Welding Punching Riveting Machining Heat Treat EDM Grinding
Shearing Crimping Laser Cut
Residual Stresses
Applied Stresses
![Page 34: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/34.jpg)
Tension Compression
Typical Residual Stress Profile following Machining, Grinding etc
0
The residual tensile manufacturing stresses are
added to the applied stresses effectively reducing the
fatigue strength of the part
Actual Stress or Load
Planned Stress or Load
![Page 35: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/35.jpg)
The surface stress ss and the depth of compression so will vary with the material properties and the peening
parameters
ss
s0
Compressive residual stresses are balanced by low magnitude and deep tensile stress
Magnitude of compressive stress s
max is at least one-half
of the material UTS.
s max
„d‟ is the depth of s max below
the surface and is proportional to the radius of the contact area
Tension Compression
Stress ( ) s
d
Typical Shot-Peening Residual Stress
Profile
0
![Page 36: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/36.jpg)
-1500
-1000
-500
0
500
1000
1500
2000
2500
0 50 100 150 200
Depth m
Ho
op
str
ess M
Pa
50/0.15/20 machined
40/0.15/10 machined
50/0.12/23 machined
50/0.15/20 peened
40/0.15/10 peened
50/0.12/23 peened
Machining stresses typically lie within 100 microns of the surface – these can be completely removed and replaced by compressive peening stresses
MACHINED
MACHINED & PEENED
Replacing Tensile Residual Stresses from
machining with Compressive Shot
Peening Stresses
![Page 37: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/37.jpg)
Fatigue life is affected by the stress amplitude and the mean stress
STRESS
CO
MPRESSIO
N
TEN
SIO
N
0
_
+
AM
PLIT
UD
E
MEAN
STRESS
Compressive Stresses close fatigue cracks over part of the cycle reducing the cycle amplitude
CYCLE
TIME
UN-SHOT PEENED
SHOT PEENED
![Page 38: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/38.jpg)
Removes manufacturing stresses Superimposes compressive stresses Combats fatigue failure Improves damage tolerance Allows higher stress levels Enhances lubrication Enables lighter design Textures surfaces Forms and corrects form errors Closes porosity in coatings and substrates Resists fretting and galling
![Page 39: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/39.jpg)
Plating
![Page 40: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/40.jpg)
Mould Texturing
![Page 41: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/41.jpg)
Prevents Stress Corrosion Cracking
![Page 42: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/42.jpg)
Peen form correction
![Page 43: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/43.jpg)
Prevents Galling of threads
Prevents Cavitation erosion
![Page 44: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/44.jpg)
Hard anodising can reduce the fatigue strength of the base
material by up to 47%,
Anodised Aluminum Bending fatigue Test
![Page 45: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/45.jpg)
Forming of
Wing skins
Peen forming Machine Form Checking Fixture
![Page 46: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/46.jpg)
0
100
200
300
400
500
600
1000 100000 10000000
Str
es
s,
MP
a
Number of cycles
Unpeened
Shot peened
→ →
→
![Page 47: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/47.jpg)
There are no Non-Destructive tests available to verify that Shot Peening has been done correctly! Positive control of the process is essential to ensure repeatability and reliability of the part.
![Page 48: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/48.jpg)
1. Media 2. Intensity 3. Coverage 4. Equipment
![Page 49: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/49.jpg)
Control Parameter 1 – Media
•size •shape •material •hardness
![Page 50: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/50.jpg)
SHAPE Shape is essential to repeat stress profile and avoid stress raisers SIZE Size consistency is essential for maintaining the depth of compressive stress
![Page 51: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/51.jpg)
Media Shape Grading
Sieved Media Distributed 360 degrees „Helter Skelter‟ Good Media Retained
![Page 52: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/52.jpg)
The Media must be inspected every:-
8 hours - steel shot
4 hours - ceramic
2 hours - glass beads
Out of specification media is removed and re-graded
Control of Shot Quality
![Page 53: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/53.jpg)
Maximum Media Size
If media is too large the radius of the part will not be protected
Diameter of media should be less than half of the minimum radius
![Page 54: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/54.jpg)
Controlled Shot Peening
Control Parameter 2 - Intensity Almen Strip System Saturation
![Page 55: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/55.jpg)
Intensity Control Almen Strips
N Strip
A Strip
C Strip
0.78 MM(0.031ins)
1.30 MM(0.051ins)
2.38 MM(0.0938ins)
Arc Height
Hardened Ball Supports Shot Stream
Almen Block
Almen Test Strip
Peening Nozzle
The Almen Strip System
Almen Strip Removed - Residual Stress Induced Curve
Digital or Dial Display
![Page 56: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/56.jpg)
![Page 57: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/57.jpg)
![Page 58: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/58.jpg)
![Page 59: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/59.jpg)
![Page 60: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/60.jpg)
![Page 61: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/61.jpg)
![Page 62: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/62.jpg)
![Page 63: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/63.jpg)
![Page 64: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/64.jpg)
Almen blocks are positioned on a dummy part or fixture in areas where intensity is to be measured
Almen strip arc height is measured at time based intervals
5 SECS
Height
12 SECS
15 SECS
19 SECS
22 SECS
7 SECS
![Page 65: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/65.jpg)
Saturation Curve
T 2T
Exposure Time
Arc
He
igh
t
10% Increase
Saturation Point
![Page 66: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/66.jpg)
~ 80% YS
Constant for material
Light SP
Effect Of Peening Intensity
Medium SP
Heavy SP
Too Heavy SP
![Page 67: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/67.jpg)
Peenstress Residual Stress
Profile Prediction Software
![Page 68: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/68.jpg)
Controlled Shot Peening
Control Parameter 3 - Coverage Peenscan Visual
![Page 69: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/69.jpg)
Visual Coverage
Partial Complete
Establishing coverage on flat surfaces and soft metals can be easily achieved under 1 x 10 magnification
![Page 70: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/70.jpg)
Peenscan Coverage
For complex shapes and hard metals the surface can be analysed by coating the surface with a flourecent tracer liquid and examining under UV (Black) light.
![Page 71: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/71.jpg)
Control Parameter 4 - Equipment Machine type Nozzles / Lances Controls (Feeds / Pressures / Flow)
![Page 72: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/72.jpg)
• Centrifugal Wheel
• Nozzle
– Gravity
– Vacuum
– Pressure
![Page 73: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/73.jpg)
Sieving Apparatus Dust Control Enclosure Control and monitoring Robotic Nozzle Manipulation
TYPICAL EQUIPMENT
![Page 74: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/74.jpg)
Lance Tooling for Narrow Slot
Deflector for small holes
Rotating Lance for Larger Bores
Reciprocating and rotating Peening lance
Peening of Hard to Reach Areas
![Page 75: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/75.jpg)
Shot Peening Callouts
• MI 230 H, 6-10A, 200%
• S 230 R, 0,15-0,25A, 200%Almen
• AF Glass, 4-6N, 100%
• Z300, 8-12A, 400%
![Page 76: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/76.jpg)
Typical Aerospace Peening Applications......
![Page 77: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/77.jpg)
3 Worldwide Facilities
• Livermore, USA
• Frederickson, USA
• Earby, UK
Support Facilities:
Livermore, CA
– Provides research & development on laser systems and programs
![Page 78: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/78.jpg)
Laser source - 600 watts Pulse – 10 - 200 nanoseconds Repetition - 6Hz Short Bursts - 2.7Hz Continuous Temperature at surface 70
oC
![Page 79: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/79.jpg)
Ablative Layer
Laser
Peening
Conventional
Shot Peening
Tamping
Layer
Plasma
Contact Time
= micro-seconds
Cold Work
10 to 50%
Contact Time
= nano-seconds
Cold Work
1 to 2%
Advantages
•Greater depths of residual compressive stress
•Less surface roughening
•Less cold work – relaxation advantages
•Targeted
•Media free
![Page 80: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/80.jpg)
Development of Square Laser beam allows the fastest possible coverage of the area. The efficiency of each individual spot is monitored in real time and can be reworked if parameters are not met.
![Page 81: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/81.jpg)
Square spots provide uniform
coverage
• Square spots provide efficient
coverage in a single treatment
layer
• Constant flat-top beam profile
provides highly uniform stress
![Page 82: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/82.jpg)
Laser peened area (both sides) Laser peening significantly extends the
fatigue lifetime of metal components
![Page 83: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/83.jpg)
-2000
-1500
-1000
-500
0
500 0 0.5 1.0
Laser Peening Shot Peening
![Page 84: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/84.jpg)
![Page 85: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/85.jpg)
![Page 86: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/86.jpg)
CASE Isotropic and vibratory polishing
Gears
Shafts
Bearings
Turbine blades
![Page 87: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/87.jpg)
Micro-pitting Progression
![Page 88: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/88.jpg)
Typical Macro-pitting
![Page 89: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/89.jpg)
C.A.S.E.
SHOT PEENED SURFACE PROFILE
SHOT PEENED AND CASE POLISHED SURFACE PROFILE
![Page 90: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/90.jpg)
C.A.S.E.
Different Profiles with Same Ra Value
Ground Grd+Peen Grd+Peen+CASE
Negative
Skew
Positive
Skew
ROUGHNESS PARAMETER
![Page 91: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/91.jpg)
Material: Case hardening Steel EN 36 (DIN : 15NiCr13 )
Surface after grinding Grinding + C.A.S.E.
C.A.S.E.
![Page 92: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/92.jpg)
Shot-Peened
C.A.S.E
Shot-Peened
+ C.A.S.E.
Extended
Process Time
Shot-Peened
+ C.A.S.E.
![Page 93: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/93.jpg)
C.A.S.E.
![Page 94: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/94.jpg)
C.A.S.E.
![Page 95: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/95.jpg)
Shot Peening
Induces compressive residual stresses from a few microns up to 0.5mm Increases fatigue strength and fatigue life Offers resistance against many fatigue failure modes Economical and well proven technology
Laser Peening
Induces 5-10 times greater depths of residual stresses than shot peening Far less cold working Less surface roughness Suitable for critical components where stresses are localised
C.A.S.E.
Reduces contact stress (micro / macro pitting) Removes surface asperities Lowers friction (reduced operating temperature and mechanical loss)
![Page 96: Neil Sheward - Metal Improvement Company, Technical Service](https://reader034.vdocuments.mx/reader034/viewer/2022042800/586d3b561a28abca518c06c3/html5/thumbnails/96.jpg)
Neil Sheward- Technical Services Manager
Metal Improvement Company
www.metalimprovement.co.uk