![Page 1: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/1.jpg)
W.D. Nix, Wadsworth Symposium
W. D. NixDepartment of Materials Science and Engineering
Stanford University
Global R&D Trends – Implications for Materials Science
Symposium Honoring Dr. Jeffrey Wadsworth2013 Acta Materialia Award in Materials and Society
March 5, 2013
Linking the challenges of materials technology with the opportunities in materials
research - an academic perspective
![Page 2: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/2.jpg)
W.D. Nix, Wadsworth Symposium
One R&D trend in materials science –in mechanical behavior
In addition to the long established problems in the discipline of structural materials:
Stiffer, Stronger, Tougher, Lighter…
We have now added: Smaller
•First motivated by needs from outside the discipline: microelectronics and functional materials
•Has led to new techniques and Ideas that now benefit a broad spectrum of science and technology
I will call this a trend
![Page 3: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/3.jpg)
W.D. Nix, Wadsworth Symposium
Mechanical behavior problems in microelectronics ~ 1983
Craig Barrett, Intel
David Barnett, StanfordBill Nix, Stanford
Consulting about mechanical reliability in metal interconnects –metal cracking
Created need to understand stresses and mechanical properties of thin films – need for new techniques and concepts
![Page 4: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/4.jpg)
W.D. Nix, Wadsworth Symposium
Nanoindenter – Pethica and Oliver - 1983
ASM meeting, Philadelphia, October 4,1983
![Page 5: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/5.jpg)
W.D. Nix, Wadsworth Symposium
Established the methodology for determining mechanical properties by nanoindentation
Google Scholar: 10,023 citations!
Most in field of Materials Science –by far!
Oliver & Pharr Method - 1992
![Page 6: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/6.jpg)
W.D. Nix, Wadsworth Symposium
Application to Low-k Dielectric FilmsNanonidentation compliant films
W.C. Oliver & G.M. Pharr, MRS Bulletin (2010)
![Page 7: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/7.jpg)
W.D. Nix, Wadsworth Symposium
Application to BiologyNanoindentation of plaques and hardening of the arteries
W.C. Oliver & G.M. Pharr, MRS Bulletin (2010)
![Page 8: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/8.jpg)
W.D. Nix, Wadsworth Symposium
MEMS Display Technology (QUALCOMM)Flat, Deformable Mirrors as Pixels for Electronic Readers
Residual stresses and mechanical properties of the glass films are crucial
![Page 9: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/9.jpg)
W.D. Nix, Wadsworth Symposium
0
100
200
300
400
500
600
700
0 500 1000 1500 2000 2500
Load
(mN
)
Displacement (nm)
Indent 1
Indent 2
Indent 3
Indent 4
Indent 5
Indent 6
Indent 7
Indent 8
Indent 9
Indent 10
Indent 11
Indent 12
Film thickness=2000 nm
Nanoindentation of a high quality glass film on Si (part of mirror-pixel structure)
Continuous stiffness: Displacement amplitude=+/- 3nm Frequency: 45 Hz
![Page 10: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/10.jpg)
W.D. Nix, Wadsworth Symposium
0
2
4
6
8
10
12
14
0 500 1000 1500 2000
Har
dnes
s (G
Pa)
Contact Depth (nm)
Indent 1Indent 2Indent 3Indent 4Indent 5Indent 6Indent 7Indent 8Indent 9Indent 10Indent 11Indent 12
Hardness and modulus of a high quality glass film on Si – substrate effect
Continuous stiffness: Displacement amplitude=+/- 3nm Frequency: 45 Hz
Film thickness=2000 nm
0
20
40
60
80
100
120
140
0 500 1000 1500 2000M
odul
us (G
Pa)
Contact Depth (nm)
Indent 1
Indent 2
Indent 3
Indent 4
Indent 5
Indent 6
Indent 7
Indent 8
Modulus of Si substrate is ~160 GPaPoisson’s Ratio=0.18
This characterization capability did not exist before 1983
![Page 11: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/11.jpg)
W.D. Nix, Wadsworth Symposium
Another newly developed technique based on an Intel-Stanford connection
![Page 12: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/12.jpg)
W.D. Nix, Wadsworth Symposium
Substrate curvature method for measuring elastic and plastic properties of thin films
Technique did not exist before the mid-1980s – led to new wave of science on the strength and plasticity of thin film materials
![Page 13: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/13.jpg)
W.D. Nix, Wadsworth Symposium
J.A. Floro, E. Chason and S.R. Lee,MRS Symposium, Fall 1995
Interest in stress measurement led to new in-situ techniques
Deposition Chamber
Substrate
He-Ne laser
Mirror
FilterLensEtalon
Glass window
CCD camera
Monitor
![Page 14: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/14.jpg)
W.D. Nix, Wadsworth Symposium
Stress Evolution in Deposited Thin Films
J.A. Floro, E. Chason, R.C. Cammarata, D.J. Srolovitz, MRS Bulletin (2002)
W on glass
V. Ramaswamy & B.M. Clemens, (2001)
-10-9-8-7-6-5-4-3-2-1012
0 20 40 60 80 100 120 140 160 180
Thickness (Å)
F/
w (
N/
m)
avg
i
160 Å W film on glassAr Pressure = 3.5 mTorr
t
avg = -0.4 GPa
i = -1.2 GPa
1
2
3
Sputter depositionA new line of research on the origins of stresses in thin films
![Page 15: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/15.jpg)
W.D. Nix, Wadsworth Symposium
What are the lessons learned?
• Useful to consider problems outside your own discipline or specialty (microelectronics, functional materials)
• Useful to look for new techniques or methods that can be used to address the new problems
NanoindentationSubstrate curvature techniques
• Connecting the new techniques to the new problems leads to new lines of research that both contribute to the solution of important problems and advance the discipline (mechanical behavior)
![Page 16: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/16.jpg)
W.D. Nix, Wadsworth Symposium
Subra Suresh’s work on Malaria
Problem: Malaria induced by P. falciparum in red blood cells; most widespread parasitic disease in humans
From research on metal fatigue and thin film mechanical properties to research on malaria!
Technique: Optical tweezers S. Henon S et al. J. Biophys (1999)Huge change in elastic rigidity
![Page 17: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/17.jpg)
W.D. Nix, Wadsworth Symposium
A new problem in the field of lithium ion batteries - decrepitation
Ionics, Vol. 6, 57-63 (2000)
K. Rhodes et al. Journal ECS (2010)
Smaller particles resist fracture – understood in terms of fracture mechanics
But problem did not attract attention until….
Nanowire electrodes synthesized!
![Page 18: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/18.jpg)
W.D. Nix, Wadsworth Symposium
The decrepitation problem and a nanowire solution
Si anode in Li+ battery Silicon is a promising anodic material
Experiences huge volume expansion and decrepitation
C. K. Chan et. al. Nature Nanotech. (2008)Is there a critical size?
Nanowire electrodes more tolerant
![Page 19: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/19.jpg)
W.D. Nix, Wadsworth Symposium
Modeling fracture using the electrochemical shock – thermal shock analogy
Lithiation Delithiation
Li+ insertion
Li+ extraction
Surfacecracking
Interiorcracking
Axis of symmetry
Axis of symmetry
I. Ryu et. al., JMPS, 2011
![Page 20: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/20.jpg)
W.D. Nix, Wadsworth Symposium
But surface cracking of crystalline Si is observed during lithiation!
![Page 21: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/21.jpg)
W.D. Nix, Wadsworth Symposium
Core-shell lithiation of Si NWs
Pressurized tube model
K. Zhao, .. Z. Suo, et al., ECS, (2012)
Si NW
1 um
Core-Shell
Crystalline Si
LixSi
PressurePartial Lith.
Tension at surface
Y (1 ln(b r))
Interface reaction controlledTwo phase core-shell
Li+
![Page 22: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/22.jpg)
W.D. Nix, Wadsworth Symposium
In-situ TEM of Si nanoparticles during lithiation
M.T. McDowell, I. Ryu, S. W. Lee et al., Advanced Materials, 2012
Fracture at surface100 nm
![Page 23: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/23.jpg)
W.D. Nix, Wadsworth Symposium
Size dependence of fracture<111> Si nanopillars
Smaller size and slow reaction prevent fracture~300 nm is critical diameter of fracture
S. W. Lee et al., PNAS, 2012
![Page 24: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/24.jpg)
W.D. Nix, Wadsworth Symposium
Lithiation of an amorphous Si nanoparticle
M.T. McDowell et al, Nano Letters (2013)
No Fracture!
![Page 25: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/25.jpg)
W.D. Nix, Wadsworth Symposium
Lithiation of amorphous Si nanopillars
No fracture observed for diameters up to a few micrometers
170 nm 650 nm 1 um
1 umPris
tine
Lith
iatio
n
1 um
L.A. Berla et al., in preparation, 2013
![Page 26: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/26.jpg)
W.D. Nix, Wadsworth Symposium
What are the lessons learned?
• Useful to consider problems outside your own discipline or specialty (electrochemistry and batteries)
• Useful to look for new techniques or methods that can be used to address the new problems
NanowiresNanopillars
• Connecting the new techniques to the new problems leads to new lines of research that both contribute to the solution of important problems and advance the discipline (mechanical behavior)
![Page 27: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/27.jpg)
W.D. Nix, Wadsworth Symposium
Conclusions• Useful to consider problems outside your own
discipline or specialty – beware of learning more and more about less and less
• Useful to look for new techniques or methods that can be used to address the new problems – they need not be “invented here”
• Connecting the new techniques to the new problems leads to new lines of research that both contribute to the solution of important problems and advance the discipline
• This style of research has become a trend in recent decades
![Page 28: Linking the challenges of materials technology with the ......Nanoindenter – Pethica and Oliver - 1983 ASM meeting, Philadelphia, October 4,1983 W.D. Nix, Wadsworth Symposium Established](https://reader035.vdocuments.mx/reader035/viewer/2022071503/6122d1a9ba70ea1dc6355456/html5/thumbnails/28.jpg)
W.D. Nix, Wadsworth Symposium
Thank you for your interest and attention
tÇw vÉÇzÜtàâÄtà|ÉÇá àÉ ]xyy