wis5 welding defects 02

55
Faisal Yusof T E C H N O L O G Y Copyright © 2003 TWI Ltd Welding Inspection Defects/Repairs Course Reference WIS 5

Upload: thang-do-minh

Post on 09-Jan-2017

506 views

Category:

Technology


64 download

TRANSCRIPT

Page 1: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Welding InspectionDefects/Repairs

Course Reference WIS 5

Page 2: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

A perfect butt weld joint, when subjected to an external force, provide a distribution of stress throughout its volume which is not significantly greater than parent metal.

DefinitionDefinition

Page 3: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

DefinitionDefinition

This is achieved as long as the following features apply :-

• Welds should consists of solid metal throughout a cross section at least equal to that of parent metal.

• All parts of a weld should be fully fused to the parent metal.

•Welds should have smoothly blended surfaces.

Page 4: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Defects which may be detected by visual inspection can be grouped under five headings

Cracks

Lack of solid metals

Lack of fusion

Lack of smoothly

blended surfaces

Miscellaneous

Weld DefectsWeld Defects

Page 5: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

CracksCracks

Page 6: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Classified by Shape Longitudinal

Transverse

Branched

Chevron

Classified by Position HAZ Centreline Crater Fusion zone Parent metal

CracksCracks Cracks that may occur in welded materials are caused generally by by many factors and may be classified by

shape and position, cracks are classed as planar.

Page 7: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Process Cracks Process Cracks

HAZ hydrogen cracking

Weld metal hydrogen cracking

Solidification cracking (Hot Tearing)

Lamellar tearing

Page 8: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

CracksCracks

HAZ hydrogen cracking Weld metal hydrogen cracking

Solidification cracking Lamellar Tearing

Page 9: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI LtdTransverse crack Longitudinal crack

Page 10: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

LACK OF SOLID METALSLACK OF SOLID METALS

Page 11: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

POROSITYPOROSITYDescription : Gas pores trapped within the weld metal

Causes :

• Damp fluxes/ corroded electrode

•Grease/hydrocarbon/water contamination of prepared surface

•Air entrapment in gas shield

•Too high arc voltage/arc length

•Incorrect/insufficient deoxidant in electrode, filler or parent metal

Preventation :

• Use dry electrodes in good condition

•Optimise gas flow

•Use electrode with sufficient deoxidation activity

•Reduce arc voltage or arc length

Page 12: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Gas CavitiesGas Cavities

Root pipingRoot piping

PorosityPorosity

Page 13: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Cluster porosity Herring bone porosity

Page 14: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Crater PipeCrater Pipe A shrinkage cavity at the end of a weld run where the arc is terminated

Causes :

•Lack of welder skill due to using processes with too high current.

•Inoperative crater filler ( GTAW )

Preventation :

• Retrain welder

•Use correct crater filling technique

Page 15: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Crater Pipe/CracksCrater Pipe/Cracks

Crater pipeCrater pipe

Crater CracksCrater Cracks

Page 16: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

RootRoot concavityconcavity

A shallow groove, which may occur in the root of a butt weld

Causes :

•Insufficient arc power to produce positive bead

•Excessive backing pressure ( GTAW )

•Lack of welder skill

•Slag flooding in backing bar groove

Preventation :

• Raise arc energy

•Reduce gas pressure

•Retraint welder

•Tilt work to prevent slag flooding

Page 17: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

root concavity

Page 18: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

UnderfillUnderfill

A weld with thickness less than that of the parent metal

Causes :

•Insufficient weld metal

•Irregular weld bead surface

Preventation :

• Increase number of weld run

•Retrain welder

Page 19: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI LtdIncomplete filled groove

Page 20: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Slag InclusionsSlag Inclusions Slag or other matters trapped during welding. The imperfection is of an irregular shape and thus differs in appearance from a gas pore

Causes :

•Heavy millscale/rust on work surface

•Incomplete slag removal from underlying surface of multipass weld

•Slag flooding ahead of the arc

•Entrapment of slag in work surface

•Unfused flux due to damage coating

Preventation :

• Grind surface prior welding

•Improve interun slag removal

•Position work to gain control of slag

•Dress work surface smooth

•Use electrode in good condition

Page 21: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Elongated slag linesInterpass slag inclusions

Page 22: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Inter- run ImperfectionsInter- run ImperfectionsIrregular along the fusion line between weld beads

Causes :

•Low arc current resulting in low fludity of weld pool

•Too high travel speed

•Inaccurate bead replacement

Preventation :

• Increase current

•Reduce travel speed

•Retrain welder

Page 23: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Lack of FusionLack of Fusion

Page 24: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Incomplete root penetrationIncomplete root penetrationFailure of the weld metal to extend into root of a joint

Causes :

•Excessively thick root face, insufficient root gap or failure to cut back sound metal in a ‘back gouging’ operation

•Low heat input

•Excessive inductance in GMAW dip transfer

•SMAW electrode too large( low current density )

•Use of vertical down welding

Preventation :

• Improved back gouging and edge preparation

•Increase arc power or decrease travel speed

•Improve electrical settings and possibly switch to spray transfer

•Reduce electrode size

•Switch to vertical up procedure

Page 25: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Root DefectsRoot Defects

Lack of root fusion Lack of root Penetration

Page 26: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Lack of root penetration Lack of root fusion

Page 27: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Lack of sidewall fusionLack of sidewall fusionLack of fusion between weld metal and parent metal at one side of weld

Causes :

•Low heat input to weld

•Molten metal flowing ahead of arc

•Oxide or scale on weld preparation

•Excessive inductance in GMAW dip transfer welding

Preventation :

•Increase arc energy or increase travel speed

•Improve electrode angle and work position

•Improve edge preparation procedure

•Reduce inductance, even if this increase spatter

Page 28: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Lack of Smoothly Lack of Smoothly Blended SurfacesBlended Surfaces

Page 29: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Surface porositySurface porosityGas pores which break the surface of the weld

Causes :

•Damp or contaminated surface of electrode

•Low fluxing activity

•Excess sulphur ( particularly free – cutting steels) producing sulphur oxide

•Loss of gas shield gas due to long arc or high breezes ( GMAW )

Preventation :

•Clean surface and dry electrodes

•Use a high activity flux

•Use high manganese to produce MnS, note free cutting should not normally be welded

•Reduce arc length

Page 30: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Excess Weld Metal ( Reinforcement )Excess Weld Metal ( Reinforcement )Reinforcement is the extra metal which produces convexity in fillet

welds and a welds thickness than the parent metal plate in butt welds.

Causes :

•Excess arc energy ( GMAW,SAW )

•Shallow edge preparation

•Faulty electrode manipulation

•Incorrect electrode size

Preventation

•Reduction of energy input

•Deepen edge preparation

•Improve welder skill

•Reduce electrode size

Page 31: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI LtdExcess cap reinforcement

Page 32: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Excessive PenetrationExcessive PenetrationProjection of the root penetration bead beyond a specified limit

Causes :

•Weld input energy too high

•Incorrect weld preparation i.e excessive root gap, thin edge preparation, lack of backing

•Use electrode unsuited to welding position

•Lack of welder skill

Preventation

•Reduce arc power/increase weld speed

•Improve work piece preparation

•Use correct electrode position

•Retrain welder

Page 33: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Excessive root penetration

Page 34: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

UndercutUndercutAn irregular groove at the toe of a run in the parent metal or in

previously deposited welding, cause by welding

Causes :

•Melting of top edge due to too high welding current ( especially at free edge) or high travel speed

•Attempting an HV fillet weld leg length

>9.0 MM

• Excessive/Incorrect weaving

•Incorrect electrode angle

Preventation

•Reduce power input,especially approaching a free edge where overheating can occur

•Weld in a flat position or use multirun technique

•Direct arc towards thicker member

Page 35: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Cap UndercutCap Undercut

Measured in both Length & DepthMeasured in both Length & Depth

Page 36: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Cap undercutRoot undercut

Page 37: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

OverlapOverlapAn Imperfection at the toe of a weld caused by metal flowing on to the

surface of the parent metal without fusing to it

Causes :

• Poor electrode manipulation

• High energy input/low travel speed causing surface flow of fillet weld

• Incorrect positioning of weld

• Electrode having too high a fluidity

Preventation

•Retrain welder

•Reduce the heat input or limit size of fillet weld to 9.0 mm leg by using multi run weld

•Change the flat position

•Change to less fluid weld metal

Page 38: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Profile DefectsProfile Defects

Poor stop/starts

Page 39: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

MiscellaneousMiscellaneous

Page 40: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

MisalignmentMisalignmentThe non – alignment of two abutting edges in a butt joint

Causes :

• Inaccuracies in assembly procedures or distortion from other welds

• Excessive ‘out of flatness' in hot rolled plate or sections

Preventation :

•Adequate checking of alignment prior to welding coupled with the use of clamps and wedges

•Check accuracy of rolled section prior to welding

Page 41: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Arc strikesArc strikesRandom areas of fused metal where the electrode, the holder, or

current return clamp accidentally touched the work and produced a short duration arc

Causes :

• Poor Access to work

• Missing insulation on electrode holder or torch

• Failure to provide an insulated resting place for the electrode holder or torch when not in use

• Loose current return clamp

Preventation :

•Improve access ( modify assembly sequence )

•Institute a regular inspection scheme for electrode holders and torches

•Provide an insulated resting place

•Regularly maintain current return clamp

Page 42: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

SpatterSpatterSmall droplets of electrode material can be projected clear of the weld

and may fused to the parent metal

Causes:

• High arc power

• Magnetic arc blow

• Incorrect setting for GMAW process

• Damp electrodes

Preventation :

•Reduce arc power

•Reduce arc length or swith to AC power

•Modify electrical settings ( but be careful to maintain full fusion

•Use dry electrodes

Page 43: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Burn ThroughBurn Through

High Amps/volts

Small Root face

Large Root Gap

Slow Travel SpeedBurn through

A localized collapse of the weld pool due to excessive penetration resulting in a hole in the root run

Page 44: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd Burn through

Burn Through

Root Defects

Page 45: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Root Coking/Oxidized Root Root Coking/Oxidized Root

Loss or insufficient back

purging gas

Most commonly occurs

when welding stainless

steels

Purging gases include

argon, helium and

occasionally nitrogen

Page 46: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Mechanical DamageMechanical Damage

Page 47: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Mechanical DamageMechanical Damage Mechanical damage can be defined as any surface material damage cause during the manufacturing process.This can included damage caused by:

Grinding

Hammering

Chiselling

Chipping

Breaking off welded attachments (torn surfaces)

Using needle guns to compress weld capping runs

Page 48: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Parent Material DefectsParent Material Defects

A welding inspector should also inspect the parent material for any visible defects

Lamination

Mechanical damage Lap

Segregation line

Page 49: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Plate LaminationPlate Lamination

Page 50: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Any Questions?Any Questions?

Page 51: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

QuestionsQuestionsQU 1. Give two main causes for the occurrence of a burn through

QU 2. Give two main causes for the occurrence of excessive root penetration on a single-V butt weld

QU 3. Give five defects, which may occur when welding carbon steel using the MMA welding process with the current setting to low

QU 4. Give three possible causes for the occurrence of lack of side wall fusion

QU 5. Sketch the following defectsa. Lack of root wall fusion b. Lack of root penetrationc. Incomplete filled groove d. Concave root

Page 52: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Weld RepairsWeld Repairs

Page 53: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

Welding RepairsWelding Repairs

Authorization for repair

Removal and preparation for repair

Testing of repair - visual and NDT

In the event of repair

Page 54: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

A weld repair may be used to improve weld profiles or extensive metal removal

Repairs to fabrication defects are generally easier than repairs to service failures because the repair procedure may be followed

The main problem with repairing a weld is the maintenance of mechanical properties

During the inspection of the removed area prior to welding the inspector must ensure that the defects have been totally removed and the original joint profile has been maintained as close as possible

Weld RepairsWeld Repairs

Page 55: Wis5 welding defects 02

Faisal Yusof

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

The specification or procedure will govern how the defective areas are to be removed. The method of removal may be

Grinding

Chipping

Machining

Filing

Oxy-Gas gouging

Arc air gouging

Weld RepairsWeld Repairs

Arc air gouging