NATIONAL CERTIFIED PIPE WELDING BUREAU WELDING PROCEDURE SPECIFICATION NO. 8-32-1 FOR GAS TUNGSTEN ARC WELDING (GTAW) AND SHIELDED METAL ARC WELDING (SMAW) OF AUSTENITIC STAINLESS STEEL PIPES, VALVES, FITTINGS AND FLANGES USING F-5 ELECTRODE WITHOUT POSTWELD HEAT TREATMENT © NCPWB This document is the property of (NCPWB Member Company Name) This Welding Procedure Specification (WPS) and Procedure Qualification Record(s) (PQR) are issued by the NCPWB for adoption by its members. Reproduction or use of this WPS and PQR(s) by anyone other than members of the NCPWB is prohibited

Upload: phungngoc

Post on 03-Feb-2018

662 views

Category:

Documents


55 download

TRANSCRIPT

  • NATIONAL CERTIFIED PIPE WELDING BUREAU

    WELDING PROCEDURE SPECIFICATION

    NO. 8-32-1

    FOR

    GAS TUNGSTEN ARC WELDING (GTAW)

    AND

    SHIELDED METAL ARC WELDING (SMAW)

    OF

    AUSTENITIC STAINLESS STEEL PIPES, VALVES, FITTINGS AND FLANGES

    USING F-5 ELECTRODE WITHOUT POSTWELD HEAT TREATMENT

    NCPWB

    This document is the property of

    (NCPWB Member Company Name)

    This Welding Procedure Specification (WPS) and Procedure Qualification Record(s) (PQR)

    are issued by the NCPWB for adoption by its members. Reproduction or

    use of this WPS and PQR(s) by anyone other than members of the NCPWB is

    prohibited

  • WELDING PROCEDURE SPECIFICATION (WPS)

    Company Name: WPS Number: 8-32-1 Original WPS Date: 3-19-75 Supporting PQRs: 87801, 87802

    Revision Number: 3 Revision Date: 10-1-13 87803, 87804

    Welding Process: Gas Tungsten Arc (GTAW) / Shielded Metal Arc (SWAW) Type: Manual

    Joints (QW-402)

    Joint Design: Single-V or U, Double-V or U, Fillets, Repairs, Build-up Details: See Typical Joint Designs

    Backing: Optional for GTAW, Required for SMAW Backing Material Type: Stainless Steel, when used

    Base Metals (QW-403) Filler Metals (QW-404) Root Balance

    P-Number: 8 Group Number: 1 Specification Number (SFA): 5.9 5.4

    to P-Number: 8 Group Number: 1 Classification: ERXXX (See below) EXXX-16 (See Below)

    Thickness Range F-number: 6 5

    Groove Welds: 1/16 to 8 A-Number: 8 8

    Fillet Welds: All Maximum Deposited Weld

    Pipe Diameter Range Metal Thickness - Groove: 8 8

    Groove Welds: >1 O.D. - Fillet: All All

    Fillet Welds: All Maximum Bead Thickness: 1/8 3/8

    Flux Trade Name: N/A N/A

    Consumable Insert: None N/A

    Positions (QW-405) Postweld Heat Treatment Technique (QW-410)

    (QW-407)

    Welding Positions: All Temp. Range: None String or Weave Bead: Either

    Welding Progression: Uphill Time Range: N/A Method of Backgouging: None

    Preheat and Interpass Electrical Initial and Interpass Cleaning: Grind to re-

    Temperature (QW-406) Characteristics move cutting oxide, solvent clean to remove

    (QW-409) cutting oil. Grind or wire brush to remove

    Minimum Preheat: 50F Current Type: DC slag or silica deposits.

    Maximum Interpass: 350F* Polarity: See Table Orifice or Gas Cup Size: #4 to #12

    Preheat Maintenance: Not Required Amperage: See Table Oscillation: N/A

    Gas (QW-408) Electrode Feed Speed: N/A Contact Tube to Work Distance: N/A

    Shielding Gas: 100% Argon Voltage: N/A Multiple or Single Pass: Either

    Composition: Welding Gr. Travel Speed: See Table Multiple or Single Electrode: N/A

    Flow Rate: 8-20 CFH Tungsten Type: 2% Thoria Peening: Not Permitted

    Gas Backing: Ar or N at Tungsten Size: 3/32, 1/8 Other:

    5-15 CFH Pulsed Current: None

    Trailing Shield: None

    Weld Layer Welding

    Process

    Filler Metal Current

    Volts

    Travel

    Speed *

    (ipm)

    Other

    Class Dia. (in) Type/Polarity Amps Base

    Metal Filler Metal

    1 GTAW As Above 3/32 or 1/8 DCSP 60-100 2-4 304 308, 308L, 316, 316L

    2 GTAW As Above 3/32 or 1/8 DCSP 70-100 2-4 304L 308L, 316, 316L

    Balance SMAW As Above 3/32 DCRP 40-80 2-4 316 316, 316L

    Balance SMAW As Above 1/8 DCRP 65-110 2-6

    316L 316L

    Balance SMAW As Above 5/32 DCRP 100-150 321,347 308L, 321

    Balance SMAW As Above 3/16 DCRP 120-190 4-8 *These values are recommended

    only, not mandatory

    The undersigned contractor, a member of the National Certified Pipe Welding Bureau, hereby adopts this

    jointly developed procedure as its company Welding Procedure Specification and certifies that this

    procedure has been qualified as shown on the attached Procedure Qualification Record.

    Contractor:

    By: Date:

    Title:

    WPS 8-32-1 NCPWB Form QW-482 4/87

    When welding different types of 300 series

    stainless to each other, select a filler metal

    designated for both types.

    For use by NCPWB members only (NCPWB)

  • September 20, 2012

    Z

    Typical Joint Designs Other joint designs shown on Engineering drawings supersede these joint details

    Butt welds

    Note 1: 1/8 inch maximum except for B31.1 and B31.5 work, 1/16 inch maximum

    Fillet, Nozzle and Branch Connection Welds

    Socket and Slip-on Flange Welds

    T = The nominal thickness of the pipe

    X = the lesser of 1.4T or the hub thickness unless another size is shown on the engineering drawings

    Y = the lesser of 1.1T or the fitting thickness unless another size is shown on the engineering drawings

    Z = for B31.9 work, minimum of the greater of the pipe nominal wall thickness or 14 in. (6 mm) and face

    fillet is not required unless specified by the design.

    3/32 to 1/8

    See note 1

    30 to 45

    3/32 to 1/8

    3/16 Nom. See Note 1

    30 to 45

    3/32 to 1/8

    1/8 min 45 min

    Smaller of T or 1/4

    X

    X

    1/16 min

    1/16 min

    Y Y

    Approximately

    1/16 before

    welding

    Size (leg)

    Dimension

    Throat

    dimension

    1/16 max

    For use by NCPWB Members Only ( NCPWB)

  • PROCEDURE QUALIFICATION RECORD (PQR)

    WPS followed during welding of test coupon: SP-313K, Rev 0 Test Date: 2-3-84

    Welding Process(s) used: Shielded Metal Arc Type: Manual

    Base Metal Specification: SA-312 type 304 to Base Metal Specification: SA-312 type 304

    P-No: 8 Group No: 1 to P-No: 8 Group No: 1 Thickness: 0.280

    Plate: Diameter if pipe: 6 Joint Type: Single V-Groove, P-8 Backing Ring, 3/16 Root Gap

    Filler Metal Specification: SFA 5.4 AWS Classification: E308-16 F-No.: 5

    A-No.: 8 Filler Metal Size: 3/32,1/8 Supplementary Filler Metal: NA

    Weld Metal Deposit Thickness : 0.280 Maximum Pass Thickness : 0.12

    Preheat Temp (F): 70 Interpass Temp (F): 350 Welding Position/Progression: 1G Rolled

    Tungsten Type/Size: NA Current: DC Polarity: RP Travel Speed: below ipm

    Postweld Heat Treatment (F): None Heat Treatment Time (Hrs): NA

    Shielding Gas Composition : NA CFH Backing Gas: NA CFH

    Stringer/Weave Bead: Weave Transfer Mode: NA

    Oscillation: NA Single/Multi-Pass: Multi Single/Multi-Arc: Single

    Layer Process Filler Class Diameter Amperage Travel Speed (ipm) Other

    1

    2

    3

    SMAW

    SMAW

    SMAW

    E308-16

    E308-16

    E308-16

    3/32

    1/8

    5/32

    90

    105

    100

    4.5

    2.5

    2.5

    Reduced Section Tensile Tests

    Specimen No. Width/Dia. Thickness Area Ult. Load (lbs) Ult. Stress (psi) Failure

    Location

    T-1 0.753 0.270 0.203 18,900 93,100 Base Metal

    T-2 0.761 0. 261 0.198 18,400 92,900 Base Metal

    Guided Bend Tests [ ] QW-452.2 (Side) [ X ] QW-462.3(a) (Trans R&F) [ ]QW-462.3(b)(Long R&F)

    Face No defects-acceptable Root No defects-acceptable

    Face No defects-acceptable Root No defects-acceptable

    Welders Name: Len Wertelet Stamp No. LM Test Number: 846988

    Welding Witnessed by : James J. Sekely Specimens Evaluated by : Earl Gallagher, PTL

    We Certify that the statements in this record are correct, and that the test coupons were prepared, welded

    and tested in accordance with the requirements of Section IX of the ASME Code.

    Contractor:

    By: Date:

    BY:

    Chairman, Technical Committee NCPWB Form QW-483 4/87 PQR Number: 87801

    For use by NCPWB members only (NCPWB)

    NATIONAL CERTIFIED

    PIPE WELDING BUREAU

  • PROCEDURE QUALIFICATION RECORD (PQR)

    WPS followed during welding of test coupon: WP-43, Rev 17, 1/21/83 PQR Number: 87802

    Welding Process(s) used: GTAW, Manual Date Test Coupon was welded: 2-11-83

    Base Metal Specification: SA-240, Type 304 to Base Metal Specification: SA-240, Type 304

    P Number: 8 Group No: 1 to P Number: 8 Group No: 1 Plate/Pipe Diameter: Plate

    Base Metal Thickne