Page 1: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Welding InspectionDefects/Repairs

Course Reference WIS 5

Page 2: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Defects which may be detected by visual inspection can be grouped under the following headings

CracksCracks

Solid inclusionsSolid inclusions

Surface and profilesSurface and profiles

Misalignment (set-up Misalignment (set-up

irregularities)irregularities)

Gas pores and porosityGas pores and porosity

Lack of fusionLack of fusion

Mechanical damageMechanical damage

Parent material damageParent material damage

MiscellaneousMiscellaneous

Page 3: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Classified by Shape Longitudinal

Transverse

Branched

Chevron

Classified by Position Classified by Position HAZHAZ CentrelineCentreline CraterCrater Fusion zoneFusion zone Parent metalParent metal

Cracks that may occur in welded materials are caused generally by many factors and may be classified by shape and position, cracks are classed as planar.

Page 4: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Hydrogen induced cold cracking Hydrogen induced cold cracking (HICC)(HICC)

Solidification cracking (Hot Tearing)Solidification cracking (Hot Tearing)

Lamellar tearingLamellar tearing

Re heat crackingRe heat cracking

Page 5: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Longitudinal parent metal crack

Longitudinal weld metal crack Lamellar tearing

Transverse weld metal crack

Page 6: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

M.S.RogersCopyright © 2003 TWI LtdTransverse crack Longitudinal crack

Page 7: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Root piping

Cluster porosityGas pore

Blow holeHerringbone porosity

Loss of gas shieldLoss of gas shield

Damp electrodesDamp electrodes

ContaminationContamination

Arc length too largeArc length too large

Damaged electrode fluxDamaged electrode flux

Moisture on parent materialMoisture on parent material

Welding current too lowWelding current too low

Gas pore <1.5mm Blow hole.>1.5mm

Page 8: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Root pipingRoot piping

PorosityPorosity

Page 9: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

M.S.RogersCopyright © 2003 TWI Ltd

Cluster porosity Herring bone porosity

Page 10: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Slag originates from welding Slag originates from welding fluxflux

MAG and TIG welding MAG and TIG welding process produce silica process produce silica inclusionsinclusions

Slag is caused by Slag is caused by inadequate cleaninginadequate cleaning

Other inclusions include Other inclusions include tungsten and copper tungsten and copper inclusions from the TIG and inclusions from the TIG and MAG welding processMAG welding process

Slag inclusions are defined as a non-metallic inclusion caused by some welding process

Slag inclusions

Parallel slag lines Lack of interun fusion + slag

Lack of sidewall fusion with

associated slag

Page 11: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

M.S.RogersCopyright © 2003 TWI Ltd

Elongated slag linesInterpass slag inclusions

Page 12: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Incomplete filled groove + Lack of sidewall fusion

12

1. Lack of sidewall fusion2. Lack of inter-run fusion

Poor welder skill

Incorrect electrode

manipulation

Arc blow

Incorrect welding

current/voltage

Incorrect travel speed

Incorrect inter-run cleaning

Page 13: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

An imperfection at the toe or root of a weld caused by metal flowing on to the surface of the parent metal

without fusing to it

ContaminationContamination

Slow travel speedSlow travel speed

Incorrect welding techniqueIncorrect welding technique

Current too lowCurrent too low

Page 14: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Toe OverlapToe OverlapFillet weldFillet weld

Toe OverlapToe OverlapButt weldButt weld

Page 15: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Incomplete root fusion

Incomplete root penetration

Low Amps/voltsLow Amps/volts

Large Root faceLarge Root face

Small Root GapSmall Root Gap

Fast Travel SpeedFast Travel Speed

Incorrect Electrode AngleIncorrect Electrode Angle

ContaminationContamination

Arc blowArc blow

Page 16: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Lack of root fusion Lack of root Penetration

Page 17: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

M.S.RogersCopyright © 2003 TWI Ltd

Lack of root penetration Lack of root fusion

Page 18: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Incomplete filled groove Poor cap profile

Excessive cap height

Poor cap profiles and excessive cap reinforcements may lead to stress concentration points at the weld toes and will also contribute to overall poor toe blend

Page 19: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

M.S.RogersCopyright © 2003 TWI Ltd

Incomplete filled grooveExcess cap reinforcement

Page 20: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Poor stop/starts

Page 21: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Spatter

Excessive currentExcessive current

Damp electrodes Damp electrodes

ContaminationContamination

Incorrect wire feed speed Incorrect wire feed speed

when welding with the MAG when welding with the MAG

welding processwelding process

Arc blowArc blow

Page 22: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Accidental striking of the arc Accidental striking of the arc

onto the parent materialonto the parent material

Faulty electrode holder Faulty electrode holder

Poor cable insulationPoor cable insulation

Poor return lead clampingPoor return lead clamping

Arc strike

Page 23: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

An irregular groove at the toe of a weld run in the parent metal

Excessive amps/voltsExcessive amps/volts

Excessive travel speedExcessive travel speed

Incorrect electrode angleIncorrect electrode angle

Excessive weavingExcessive weaving

Incorrect welding techniqueIncorrect welding technique

Electrode too largeElectrode too large

Page 24: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Measured in both Length & DepthMeasured in both Length & Depth

Page 25: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

M.S.RogersCopyright © 2003 TWI Ltd

Cap undercutRoot undercut

Page 26: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Shrinkage groove

Insufficient weld metal Insufficient weld metal deposited in the root passdeposited in the root pass

Too fast a cooling rate during Too fast a cooling rate during the application of the root the application of the root bead passbead pass

Poor welding techniquePoor welding technique

A shallow groove caused by contraction in the weld metal along each side of the penetration bead

Page 27: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Concave root

Root faces too largeRoot faces too large

Root gap too largeRoot gap too large

Excessive back purge pressure Excessive back purge pressure during TIG weldingduring TIG welding

Excessive root bead grinding Excessive root bead grinding before the application of the before the application of the second passsecond pass

A shallow groove, which may occur in the root of a butt weld

Page 28: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Page 29: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Excessive root penetration

Root faces too smallRoot faces too small

Root gap too largeRoot gap too large

Excessive amps/voltsExcessive amps/volts

Slow travel speedSlow travel speed

Root penetration bead in excess in accordance with the relevant specification being used

Page 30: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Page 31: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

M.S.RogersCopyright © 2003 TWI Ltd

Concave root Excessive root penetration

Page 32: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

High Amps/voltsHigh Amps/volts

Small Root faceSmall Root face

Large Root GapLarge Root Gap

Slow Travel SpeedSlow Travel SpeedBurn through

A localized collapse of the weld pool due to excessive penetration resulting in a hole in the root run

Page 33: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Burn through

Burn Through

Page 34: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Loss or insufficient back Loss or insufficient back

purging gaspurging gas

Most commonly occurs Most commonly occurs

when welding stainless when welding stainless

steelssteels

Purging gases include Purging gases include

argon, helium and argon, helium and

occasionally nitrogen occasionally nitrogen

Page 35: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Crater pipeCrater pipe

Weld craterWeld crater

Page 36: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Crater pipe is a shrinkage defect and not a gas defect, it has the appearance of a gas pore in the weld crater

Too fast a cooling rateToo fast a cooling rate

Deoxidization Deoxidization

reactions and liquid to reactions and liquid to

solid volume changesolid volume change

ContaminationContamination

Crater cracksCrater cracks(Star cracks)(Star cracks)

Crater pipeCrater pipe

Page 37: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Mechanical damage can be defined as any surface material damage cause during the manufacturing process.This can included damage caused by:

Grinding

Hammering

Chiselling

Chipping

Breaking off welded attachments (torn surfaces)

Using needle guns to compress weld capping runs

Page 38: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

A variation of leg lengths on a fillet weld

Note: Unequal leg lengths on a fillet weld may be specified as part of the design, in which case it will not be considered as a defect.

Page 39: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Plate/pipe Linear Misalignment (Hi-Lo)

Angular Misalignment

Linear misalignment is measured from the lowest plate to the highest point of the cap

Angular misalignment is measured in degrees

Page 40: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

mm

Page 41: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

QU 1. Give two main causes for the occurrence of a burn through

QU 2. Give two main causes for the occurrence of excessive root penetration on a single-V butt weld

QU 3. Give five defects, which may occur when welding carbon steel using the MMA welding process with the current setting to low

QU 4. Give three possible causes for the occurrence of lack of side wall fusion

QU 5. Sketch the following defectsa. Lack of root wall fusion b. Lack of root penetrationc. Incomplete filled groove d. Concave root

Page 42: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

All materials arriving on site should be inspected for:

Size / dimensions

Condition

Type / specification

In addition other elements may need to be considered depending on the materials form or shape

Page 43: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Parent material defects include:

Lamination

Mechanical damage Lap

Segregation line

Laminations are caused in the parent plate by the steel making process, originating from ingot casting defects.Segregation bands occur in the centre of the plate and are low melting point impurities such as sulphur and phosphorous.Laps are caused during rolling when overlapping metal does not fuse to the base material.

Page 44: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Page 45: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

Authorization for repair

Removal and preparation for repair

Testing of repair - visual and NDT

In the event of repairIn the event of repair

Page 46: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

A weld repair may be used to improve weld profiles or A weld repair may be used to improve weld profiles or extensive metal removalextensive metal removal

Repairs to fabrication defects are generally easier than Repairs to fabrication defects are generally easier than repairs to service failures because the repair procedure may repairs to service failures because the repair procedure may be followedbe followed

The main problem with repairing a weld is the maintenance The main problem with repairing a weld is the maintenance of mechanical propertiesof mechanical properties

During the inspection of the removed area prior to welding During the inspection of the removed area prior to welding the inspector must ensure that the defects have been totally the inspector must ensure that the defects have been totally removed and the original joint profile has been maintained removed and the original joint profile has been maintained as close as possible as close as possible

Page 47: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

The specification or procedure will govern how the defective areas are to be removed. The method of removal may be

GrindingGrinding

ChippingChipping

MachiningMachining

FilingFiling

Oxy-Gas gougingOxy-Gas gouging

Arc air gougingArc air gouging

Page 48: Weld Defects- Repairs

19 Sep 0219 Sep 02 M.S.Rogers

T E

C H

N O

L O

G Y

Copyright © 2003 TWI Ltd

WI 3.1

QU 1. State six points of importance of repair welding.

QU 2. State two NDT methods that may be applied to a repair in a weld

QU 3. State three documents, which the inspector should refer to when carrying out repairs.

QU 4. In some cases why might a specification not allow a crack to be repaired, regardless of size and orientation?