technol mh / mis / ms / ml98 technol mh, mis, ms and ml98 are derived from fully hydrogenated castor...
TRANSCRIPT
Technol MH / MIS / MS / ML98
Technol MH, MIS, MS and ML98 are derived from Fully Hydrogenated Castor Oil that was developed and manufactured for the raw material, especially for the cosmetics.
Castor Oil has unique structure. It has 3 hydroxyl groups in the molecule (and 1 ether bond).
Due to this unique structure and high safety characters, Castor Oil is well known and used as raw material for the cosmetics for a long time. It is perform high viscosity and get to fit the pigment and dye.
We apply unique characters of Castor Oil to Technol MH, MIS, MS and ML98 and developed from the following viewpoints;
Improve the character of hydrogenated castor oil. Hydrogenated Castor Oil is stable to oxidation. But too hard and
easy to crystallization. Castor Oil has unique structure.
Technol MH / MIS / MS / ML98
Character
High Polarity Oil
High Stability to Oxidation
Application
Glossy, semitransparent paste
High dispersion force of pigment
Increase rich feeling to cream
Increase gloss
Foundation
Hair pack
Technol MH
INCI NAME Hydrogenated Castor Oil Hydroxystearate
JCID (Japan) 508125
CAS No. -
EINECS No. -
Technol MIS
INCI NAME Hydrogenated Castor Oil Isostearate
JCID (Japan) 505014
CAS No. -
EINECS No. -
Technol MS
INCI NAME Hydrogenated Castor Oil Stearate
JCID (Japan) 504201
CAS No. -
EINECS No. -
Technol ML98
INCI NAME Hydrogenated Castor Oil Laurate
JCID (Japan) -
CAS No. 85711-76-8
EINECS No. 288-338-7
Types
Structure
CH2
CH
O
O
O
C
O
(CH2)10 CH
OH
(CH2)5CH3CH2
C (CH2)10 CH
OH
(CH2)5CH3
O
C
O (CH2)10 CH
OH
(CH2)5CH3
CH
O
(CH2)5CH3
C
O
(CH2)10
Technol MH
Hydrogenated Castor Oil Hydroxystearate
12-Hydroxystearic acid
Structure
Technol MIS
Hydrogenated Castor Oil Isostearate
Isostearic acid
CH2
CH
O
O
O
C
O
(CH2)10 CH
OH
(CH2)5CH3CH2
C (CH2)10 CH
OH
(CH2)5CH3
O
C
O
CH
O
(CH2)5CH3
C
O
C17H35
(CH2)10
Structure
Technol MS
Hydrogenated Castor Oil Stearate
Stearic acid
CH2
CH
O
O
O
C
O
(CH2)10 CH
OH
(CH2)5CH3CH2
C (CH2)10 CH
OH
(CH2)5CH3
O
C
O
CH
O
(CH2)5CH3
C
O
(CH2)16CH3
(CH2)10
Structure
Technol ML98
Hydrogenated Castor Oil Laurate
Lauric acid
CH2
CH
O
O
O
C
O
(CH2)10 CH
OH
(CH2)5CH3CH2
C (CH2)10 CH
OH
(CH2)5CH3
O
C
O
CH
O
(CH2)5CH3
C
O
(CH2)10CH3
(CH2)10
Specification
Trade Name Technol MH Technol MIS Technol MS Technol ML98
Appearance Pale Yellow Paste Slightly Smell
Acid Value 6.0Max 6.0Max 6.0Max 6.0Max
Saponification Value 175.0-195.0 175.0-195.0 175.0-195.0 190.0-210.0
Hydroxyl Value 100.0-130.0 70.0-95.0 70.0-95.0 70.0-95.0
Iodine Value 10.0Max 8.0Max 8.0Max 8.0Max
Melting Point(℃) - 43.0-48.0 40.0-55.0 -
Heavy Metal 20ppmMax 20ppmMax 20ppmMax 20ppmMax
Arsenic 2ppmMax 2ppmMax 2ppmMax 2ppmMax
Residue on Ignition (%) 0.50Max 0.10Max 0.5Max 0.5Max
Loss on Drying (%) 2.0Max 1.0Max 1.0Max 2.0Max
Package Net 16kg Tin Can
Physical Characteristics
Trade Name Technol MH Technol MIS Technol MS Technol ML98
Index of Refraction
(60℃) 1.454 1.453 1.451 1.450
Viscosity (mPa・
s, 60℃) 190 118 124 109
Specific Gravity (80℃) 0.898 0.892 0.897 0.904
Viscosity & Refractive Index
1 10 100 1000 1.43
1.44
1.45
1.46
1.47
1.48
1.49
Ref
ract
ive
Inde
x (a
t60 ℃
)
Viscosity-Refractive Index
Viscosity(mPa・s at60℃)
.
Lanolin
Special Grade Lanolin
MH MIS
Castor oil
MS ML98
Hydration Force
0
50
100
150
200
250
300
350
400
450
%
MH MIS MS ML98 Lanolin LiquidLanolin
SpecialGrade
Lanoline
Castor Oil Vaseline
Only Product Product:Vaseline=1:1
Dropping refined water to 10 grams of controls and knead. When refined water does not into controls, it is the end point. And indicates by percentage to controls.
Dispersion Force Of Pigment
Zinc Oxide
0 10 20 30 40 50 60 70 80 90 100
Liquid ParaffinVaseline
Castor OilCamellia Oil
Special Grade LanolineLiquid Lanolin
LanolinML98
MSMISMH
%Only Product Product:Liquid Paraffin=1:1
← Good Bad →
Dropping controls(*1) to 3 grams of powder pigment(*2) and stir by spatula. When as a whole of materials turn into lump (cake), it is the end point. And indicates by percentage to powder pigment.*1 : Blanc Technol MH, MIS, MS and ML98 or mixture by even MH (or MIS or MS or ML98) liquid paraffin.*2 : Zinc Oxide MZO-25
Dispersion Force Of Pigment
Titanium Oxide
0 10 20 30 40 50 60 70 80 90 100
Liquid ParaffinVaseline
Castor OilCamellia Oil
Special Grade LanolineLiquid Lanolin
LanolinML98
MSMISMH
%Only Product Product:Liquid Paraffin=1:1
← Good Bad →
Dropping controls(*1) to 3 grams of powder pigment(*2) and stir by spatula. When as a whole of materials turn into lump (cake), it is the end point. And indicates by percentage to powder pigment.*1 : Blanc Technol MH, MIS, MS and ML98 or mixture by even MH (or MIS or MS or ML98) liquid paraffin.*2 : Titanium Oxide CR-50
Dispersion Force Of Pigment
← Good Bad →
Sericite
0 10 20 30 40 50 60 70 80 90 100
Liquid Paraffin
Vaseline
Castor Oil
Camellia Oil
Special Grade Lanoline
Liquid Lanolin
Lanolin
ML98
MS
MIS
MH
%Only Product Product:Liquid Paraffin=1:1
Dropping controls(*1) to 3 grams of powder pigment(*2) and stir by spatula. When as a whole of materials turn into lump (cake), it is the end point. And indicates by percentage to powder pigment.*1 : Blanc Technol MH, MIS, MS and ML98 or mixture by even MH (or MIS or MS or ML98) liquid paraffin.*2 : Celicite SE
Solubility
Ethanol Acetone Liquid Paraffin Castor Oil Camellia Oil
r.t. Heating r.t. Heating r.t. Heating r.t. Heating r.t. Heating
MH10% S S S S D S S S D S1:
1D S S S D S D S I S
MIS10% D S S S S S S S S S1:
1S S D S D S D S D S
MS10% D S S S S S S S S S1:
1S S D S D S D S D S
ML9810% S S S S S S S S D S1:
1S S I S D S D S D S
Triethyl Hexanoin Glycerol Vaseline Dimethicone 10CS
r.t. Heating r.t. Heating r.t. Heating r.t. Heating
MH10% D S I I - S I I1:
1D S I I - S I I
MIS10% S S I I - S I I1:
1D S I I - S I I
MS10% S S I I - S I I1:
1D S I I - S I I
ML9810% D S I I - S I I1:
1D S I I - S I I
r.t. : Room temperature S : Soluble D : Dispersion I : Insoluble
Test Sample Weight: 5g10%=10% of MH or MIS or MS or ML98=10%/5g: 90%/5g of Solvents, 1:1=MH or MIS or MS or ML98: Solvents or Oils=50%: 50%Watching solubility at room temperature and heating. (Melting or dissolving point)
Oxidation Stability
CDM Test ;Measurement equipment used the Rancimat743 and measured it on condition that the temperature of 120 , and air flux 20 L/h.℃
Induction timeStability time
0
10
20
30
40
50
60
10 20 30 40 50 60 70
µS
/c
m
h
Castor Oil / 020808A MH / E150402 MIS / E150502
ML98 / E161101 MS / E161102
Castor Oil
MHMISMSML98
谢谢您了