stress corrosion cracking

50
CANMET- MTL 1 Metallurgical Factors in Stress Corrosion Cracking (SCC) and Hydrogen-Induced Cracking (HIC) Metallo-2007 Indian Institute of Technology, Kanpur in Honour of Professor T. R. Anantharaman Winston Revie and Mimoun Elboujdaini CANMET Materials Technology Laboratory Natural Resources Canada, Ottawa, Canada December 10, 2007

Upload: ssjuned

Post on 02-Oct-2015

10 views

Category:

Documents


1 download

DESCRIPTION

? Hydrogen-Induced Cracking (HIC)- Metallurgical and Environmental Variables- Inclusions? Stress Corrosion Cracking (SCC)- Metallurgical, Mechanical, Environmental,and Electrochemical Variables- Inclusions? Conclusions? What Does the Future Hold?? Collaboration/A World without Borders? Acknowledgements

TRANSCRIPT

  • CANMET-MTL

    1

    Metallurgical Factors in Stress Corrosion Cracking (SCC) and Hydrogen-Induced Cracking (HIC)Metallo-2007Indian Institute of Technology, Kanpurin Honour of Professor T. R. Anantharaman

    Winston Revie and Mimoun ElboujdainiCANMET Materials Technology LaboratoryNatural Resources Canada, Ottawa, Canada

    December 10, 2007

  • CANMET-MTL

    2

  • CANMET-MTL

    3

    Outline Overview of Underground Oil and Gas Pipelines Hydrogen-Induced Cracking (HIC)

    - Metallurgical and Environmental Variables- Inclusions

    Stress Corrosion Cracking (SCC)- Metallurgical, Mechanical, Environmental,

    and Electrochemical Variables- Inclusions

    Conclusions What Does the Future Hold? Collaboration/A World without Borders Acknowledgements

    I

    n

    s

    i

    d

    e

    O

    u

    t

    s

    i

    d

    e

  • CANMET-MTL

    4

  • CANMET-MTL

    5

    Underground Pipeline2 Sides to Every Pipe

    Soil, Microorganisms,Unstable Terrain

    Flowing Oil, Gas, Brine

    Steel, Coating

    Flowing Oil, Gas,

    Brine

  • CANMET-MTL

    6

    HIC in Steel Exposed to Sour Gas

  • CANMET-MTL

    7

    Hydrogen-InducedCracking (HIC)

    Internal cracks caused by trapped hydrogen atoms.- Cracks parallel to

    rolling plane. - Residual or applied

    tensile stress not necessary for HIC.

  • CANMET-MTL

    8

    Prediction of HIC

    1. Immersion, 4 days, in H2S-satd buffer solution, pH varied from 1.1 to 5.9

    2. Diffusible hydrogen measured, glycerol displacement at 45oC

    3. Coupons examined for cracking, ultrasonic C-scan, metallographic examination

  • CANMET-MTL

    9

    pHth and CHth

    Environment pHth Lowest pH at which no HIC was

    detected

    Material CHth Highest hydrogen concentration in

    the steel at which no HIC was detected

  • CANMET-MTL

    10

    Criterion for HIC

    0

    0 LH

    cHth

    cH0

    cH0H2S/H2O

    Steel

    AirHIC

    0

    cH0 Concentration of H at the inner pipe surfacecHth Threshold H Concentration

    No HIC

  • CANMET-MTL

    11

    Criterion for HIC

    HIC occurs if:

    cH0 > cHth

    Environmental MaterialVariable Variable

  • CANMET-MTL

    12

  • CANMET-MTL

    13

    Title

    0

    0.5

    1

    1.5

    2

    2.5

    0 0.1 0.2 0.3 0.4 0.5Volume fraction of inclusions (%)

    .

    T

    h

    r

    e

    s

    h

    o

    l

    d

    h

    y

    d

    r

    o

    g

    e

    n

    c

    o

    n

    c

    e

    n

    t

    r

    a

    t

    i

    o

    n

    (

    m

    L

    )

    .

    Volume Fraction of Inclusions, %

    T

    h

    r

    e

    s

    h

    o

    l

    d

    H

    y

    d

    r

    o

    g

    e

    n

    C

    o

    n

    c

    e

    n

    t

    r

    a

    t

    i

    o

    n

    ,

    m

    L

    HIC and Inclusions

  • CANMET-MTL

    14

    Inclusions Inclusions in cracks are MnS, by EDX Provide sites for H to accumulate

    Steel Crack Ca/SA Yes 0.15B Yes 0.50C Yes 0.96D Yes 1.31E No 2.62F No 2.50

    Optimum Ca/S Ratio2

  • CANMET-MTL

    15

    Microstructures

  • CANMET-MTL

    16

  • CANMET-MTL

    17

    Stress Corrosion Cracking Is

    A cracking process that requiresthe simultaneous action of acorrosive and a sustained tensilestress.

  • CANMET-MTL

    18

    Requirements

    1.Steel susceptible to SCC2.Tensile stress3.Potent environment

    - Coating failure provides access of aqueous environment to pipe surface.

  • CANMET-MTL

    19

    Stress

    Hoop stress- from internal pipe pressure

    Axial stress- from soil movement or localized pipe bending

    Residual stress - from pipe forming or steel making operations

    Cyclic stress- Fluctuations in operating pressure

  • CANMET-MTL

    20

    From: N.E.B Report on SCC, MH-2-96 (1996)

    Stresses in Pipelines

  • CANMET-MTL

    21

  • CANMET-MTL

    22

    Types of SCC

    Near-Neutral-pH SCC- Transgranular

    High-pH SCC- Intergranular

    Orientation:- Longitudinal- Circumferential

  • CANMET-MTL

    23

    Stages of SCC

    1. Generation of Environment2. Initiation of SCC3. Propagation of SCC

  • CANMET-MTL

    24

    Development of 5 cracks, a, b, c, d and e, after the total exposure time shown, in X-65, max = 70% YS, R = 0.4 and f = 1 Hz in NS4 solution saturated with CO2, showing the correlation of crack initiation, pits and non-metallic inclusions and the interaction and coalescence of cracks. (Observations were made on replicas.)

    e

    d

    c

    b

    aa

    b

    c

    d

    e

    a

    b

    cd

    e

    a

    b

    c

    d

    e

    b

    c

    d

    e

    a

    Total Exposure Time 309 h

    469 h747 h 1025 h

    300 m

    20 m

  • CANMET-MTL

    25

    200 m

    a

    b

    c

    e

    a

    b

    c

    e

    (a) (b)

    N = 2.69 x 106 CyclesN = 1.69 x 106 Cycles

    20

    dd

    469 h 747 h

  • CANMET-MTL

    26

    EDX Spectrum Before Test After Test

    (a)

    (b)

    (c)

    CaAl

    O

    S

    20 m

    O

    AlS Ca

    Al

    O

    Ca

    S Ca

    Ca

    Ca

    S

    S

    Al

    Al

    Al-oxide

    CaAlO3dark

    CaS

    CaS

    All dissolved

    EDS spectra and the morphologies associated with three inclusions in a X-65 steel sample before and after test at max= 90%YS, R=0.6 and f=0.1Hz in NS-4 solution saturated with N2/5%CO2. Note: Effect of S on corrosion around inclusions.

  • CANMET-MTL

    27

    Schematic of Inclusion

    Sulfide, (soluble)

    Oxide (insoluble)

    In some cases, CaS envelopes oxide/aluminate inclusion.Aluminate inclusions have poor deformability, remain spherical.In polishing to 1 m diamond finish, use non-aqueous lubricant, oil-based diamond.

  • CANMET-MTL

    28

  • CANMET-MTL

    29

    Focused ion beam images of crack in X-65 specimen after 4.15 x 106cycles, max = 70% YS, R = 0.4, f = 1 Hz, NS-4 solution, CO2 satd. (a) Plan view of crack, FIB secondary electron image, tilt 0 deg. (b) Enlargement of crack tip area in ion-milled cross-sectioned region, tilt 30 deg. (b) image in secondary ion mode,

    (a)

    X 25 m Y 25 m

  • CANMET-MTL

    30

    WrappedNot Wrapped

    X-65 steel, max = 70% YS, R = 0.4, f = 1 Hz, in NS4 solution saturated with CO2. Right part of specimen in (a) was coated with PTFE film during the test interval between 469 and 747 h. No coating between the exposure of 747 and 1025 h (b).

    747 h 1025 h

  • CANMET-MTL

    31

    Pipe Fatigue Precracking

  • CANMET-MTL

    32

    Full-Scale Pipe Test for SCC

  • CANMET-MTL

    33

  • CANMET-MTL

    34

    Conclusions - 11. SCC promoted by:

    1. Decreasing R (min./max. stress)2. Increasing frequency

    2. Environment that leads to SCC is generated by the balance between:

    CO2CP current

    3. Inclusions provide initiation sites for pitting4. Pits provide initiation sites for SCC5. Proximity of several small cracks can lead to

    linkage

  • CANMET-MTL

    35

    Conclusions 2

    6. SCC Initiation SitesPitsInclusionsSurface geometric discontinuitiesCoating Disbondments

  • CANMET-MTL

    36

    Conclusions 3

    7. Elongated inclusions provide H trap sites for HIC initiation

    1. Good correlation between inclusion measurements and HIC

    2. Lower volume fraction of inclusions ~ increased HIC resistance

    3. Banded microstructure decreases HIC resistance

  • CANMET-MTL

    37

    What is the Main Question about Corrosion?

    1. Will there be another failure? If?

    2. When will the next failure occur? When?

    3. Where will the next failure occur? Where?

    What do YOU think?

  • CANMET-MTL

    38

  • CANMET-MTL

    39

    100 Years of Corrosion R&D The Foundation

    Sensors for Field Measurements

    Instrumentation for Data Collection

    Software for Data Analysisand Decision-making

    Cellular Network/Satellite Communications

    Information on Data & Decisions

    Building on Success

  • CANMET-MTL

    40

    Intelligent Systems Are Built on

    1. Knowledge of Corrosion2. Sensors3. Instrumentation4. Software5. Remote Communications

    1960s: Design Corrosion Out2000s: Design Smart Systems for Corrosion Monitoring and

    Decision-makingMonitoring online, in real time, all the time

    Convergence of technologies provides new opportunities to manage corrosion.

  • CANMET-MTL

    41

  • CANMET-MTL

    42

  • CANMET-MTL

    43

    Corrosion Control Wagon

    $$$

  • CANMET-MTL

    44

    A Strategy Meeting

    Corrosion Control Wagon

    $$$

  • CANMET-MTL

    45

    Corrosion Control Wagon

    Team Leader

    $$$

  • CANMET-MTL

    46

    Acknowledgements

    Jenny Been Mahmoud ShehataJenny Jackman Yong-zhi WangDave Kiff Glenn WilliamsYves Lafrenire Wenyue ZhengRuel Ramsingh

    GRIPRCICanadian Federal Interdepartmental

    Program of Energy R&D (PERD)

  • CANMET-MTL

    47

    Last Thought

    Managing corrosion is an investment in asset protection that should result in cost savings because, when corrosion is managed, the cost of failure by corrosion is saved.

  • CANMET-MTL

    48

    Knowing is not enough; we must apply.

    Willing is not enough; we must do.

    Goethe

    Failure Prevention

  • CANMET-MTL

    49

    NS-4 Solution

    483 mg/L NaHCO3 122 mg/L KCl 137 mg/L CaCl2 131 mg/L MgSO47H2O

    Trang Web nay coi cung hay, vao coi thu di http://gaigoibaucat.xlphp.net

    unTrang Web nay coi cung hay, vao coi thu di http://gaigoibaucat.xlphp.net

  • CANMET-MTL

    50

    Trang Web nay coi cung hay, vao coi thu di http://gaigoibaucat.xlphp.net

    C:\WINDOWS\hinhem.scr