re-aluminizing of 60cm mirror at maidanak observatory kiichi okita*, takashi ito**, fumi yoshida**,...
TRANSCRIPT
![Page 1: Re-aluminizing of 60cm mirror at Maidanak Observatory Kiichi Okita*, Takashi Ito**, Fumi Yoshida**, Seitaro Urakawa***, Kenshi Yanagisawa*, Daisuke Kuroda*,](https://reader036.vdocuments.mx/reader036/viewer/2022062421/56649cad5503460f949702fa/html5/thumbnails/1.jpg)
Re-aluminizing of 60cm mirror at Maidanak Observatory
Kiichi Okita*, Takashi Ito**, Fumi Yoshida**, Seitaro Urakawa***, Kenshi Yanagisawa*, Daisuke Kuroda*, Hisashi Koyano*, Eiji Kanbe*, Shinobu Ozaki**(* Okayama Astrophysical Observatory of NAOJ, **NAOJ, ***Spaceguard)
2nd Maidanak Observatory Users Meeting 2010.6.22
Date : 2010. 4. 12, 13
Done by : K.Okita, K.Yanagisawa, D.Kuroda, H.Koyano, E.Kanbe (Okayama) T. Ito, F. Yoshida, S. Urakawa (Asteroid group)
![Page 2: Re-aluminizing of 60cm mirror at Maidanak Observatory Kiichi Okita*, Takashi Ito**, Fumi Yoshida**, Seitaro Urakawa***, Kenshi Yanagisawa*, Daisuke Kuroda*,](https://reader036.vdocuments.mx/reader036/viewer/2022062421/56649cad5503460f949702fa/html5/thumbnails/2.jpg)
Re-Aluminizing sequence 1. Wash by water 2. Remove old aluminum by Sodium hydroxide(NaOH) 3. Polish by Sodium Hydrogen Carbonate ( 2NaHCO 3 ) 4. Wipe by cotton cloth with alcohol 5. Install mirror in the Vacuum chamber 6. Pumping vacuum camber into 5X10-6 torr. (Use the cryio-pump & the Meissner-coil pump) 7. Ion-bombardment (3X10-2 torr 20min.) 8. One more Pumping vacuum camber into 5X10-6 torr. (Use the cryio-pump & the Meissner-coil pump) 9. Spatter aluminum (6 times X 6 filaments about 30min.) 10. Take out mirrors from chamber 11. Packing mirror to transportation box.
![Page 3: Re-aluminizing of 60cm mirror at Maidanak Observatory Kiichi Okita*, Takashi Ito**, Fumi Yoshida**, Seitaro Urakawa***, Kenshi Yanagisawa*, Daisuke Kuroda*,](https://reader036.vdocuments.mx/reader036/viewer/2022062421/56649cad5503460f949702fa/html5/thumbnails/3.jpg)
60cm mirror (before re-aluminizing) 50cm mirror (before re-aluminizing)
Small mirrors (before re-aluminizing) Remove levels
![Page 4: Re-aluminizing of 60cm mirror at Maidanak Observatory Kiichi Okita*, Takashi Ito**, Fumi Yoshida**, Seitaro Urakawa***, Kenshi Yanagisawa*, Daisuke Kuroda*,](https://reader036.vdocuments.mx/reader036/viewer/2022062421/56649cad5503460f949702fa/html5/thumbnails/4.jpg)
Re-Aluminizing sequence 1. Wash by water 2. Remove old aluminum by Sodium hydroxide(NaOH) 3. Polish by Sodium Hydrogen Carbonate ( 2NaHCO 3 ) 4. Wipe by cotton cloth with alcohol 5. Install mirror in the Vacuum chamber 6. Pumping vacuum camber into 5X10-6 torr. (Use the cryio-pump & the Meissner-coil pump) 7. Ion-bombardment (3X10-2 torr 20min.) 8. One more Pumping vacuum camber into 5X10-6 torr. (Use the cryio-pump & the Meissner-coil pump) 9. Spatter aluminum (6 times X 6 filaments about 30min.) 10. Take out mirrors from chamber 11. Packing mirror to transportation box.
![Page 5: Re-aluminizing of 60cm mirror at Maidanak Observatory Kiichi Okita*, Takashi Ito**, Fumi Yoshida**, Seitaro Urakawa***, Kenshi Yanagisawa*, Daisuke Kuroda*,](https://reader036.vdocuments.mx/reader036/viewer/2022062421/56649cad5503460f949702fa/html5/thumbnails/5.jpg)
Wash, wash ! Remove old-aluminum by NaOH(10%)
Polishing by Sodium Hydrogen Carbonate
![Page 6: Re-aluminizing of 60cm mirror at Maidanak Observatory Kiichi Okita*, Takashi Ito**, Fumi Yoshida**, Seitaro Urakawa***, Kenshi Yanagisawa*, Daisuke Kuroda*,](https://reader036.vdocuments.mx/reader036/viewer/2022062421/56649cad5503460f949702fa/html5/thumbnails/6.jpg)
Re-Aluminizing sequence 1. Wash by water 2. Remove old aluminum by sodium hydroxide(NaOH) 3. Polish by Sodium Hydrogen Carbonate ( 2NaHCO 3 )
4. Wipe by cotton cloth with alcohol 5. Install mirror in the Vacuum chamber 6. Pumping vacuum camber into 5X10-6 torr. (Use the cryio-pump & the Meissner-coil pump) 7. Ion-bombardment (3X10-2 torr 20min.) 8. One more Pumping vacuum camber into 5X10-6 torr. (Use the cryio-pump & the Meissner-coil pump) 9. Spatter aluminum (6 times X 6 filaments about 30min.) 10. Take out mirrors from chamber 11. Packing mirror to transportation box.
![Page 7: Re-aluminizing of 60cm mirror at Maidanak Observatory Kiichi Okita*, Takashi Ito**, Fumi Yoshida**, Seitaro Urakawa***, Kenshi Yanagisawa*, Daisuke Kuroda*,](https://reader036.vdocuments.mx/reader036/viewer/2022062421/56649cad5503460f949702fa/html5/thumbnails/7.jpg)
Wipe mirrors using cotton cloth with alcohol
![Page 8: Re-aluminizing of 60cm mirror at Maidanak Observatory Kiichi Okita*, Takashi Ito**, Fumi Yoshida**, Seitaro Urakawa***, Kenshi Yanagisawa*, Daisuke Kuroda*,](https://reader036.vdocuments.mx/reader036/viewer/2022062421/56649cad5503460f949702fa/html5/thumbnails/8.jpg)
Re-Aluminizing sequence 1. Wash by water 2. Remove old aluminum by Sodium hydroxide(NaOH) 3. Polish by Sodium Hydrogen Carbonate ( 2NaHCO 3 ) 4. Wipe by cotton cloth with alcohol
5. Install mirror in the Vacuum chamber 6. Pumping vacuum camber into 5X10-6 torr. (Use the cryio-pump & the Meissner-coil pump) 7. Ion-bombardment (3X10-2 torr 20min.) 8. One more Pumping vacuum camber into 5X10-6 torr. (Use the cryio-pump & the Meissner-coil pump) 9. Spatter aluminum (6 times X 6 filaments about 30min.) 10. Take out mirrors from chamber 11. Packing mirror to transportation box.
![Page 9: Re-aluminizing of 60cm mirror at Maidanak Observatory Kiichi Okita*, Takashi Ito**, Fumi Yoshida**, Seitaro Urakawa***, Kenshi Yanagisawa*, Daisuke Kuroda*,](https://reader036.vdocuments.mx/reader036/viewer/2022062421/56649cad5503460f949702fa/html5/thumbnails/9.jpg)
Set-up mirrors in the Vacuum Chamber Lock the mirrors by chuck
Closing the chamber 60cm mirror
60cm
50cm
20cm 15cm
![Page 10: Re-aluminizing of 60cm mirror at Maidanak Observatory Kiichi Okita*, Takashi Ito**, Fumi Yoshida**, Seitaro Urakawa***, Kenshi Yanagisawa*, Daisuke Kuroda*,](https://reader036.vdocuments.mx/reader036/viewer/2022062421/56649cad5503460f949702fa/html5/thumbnails/10.jpg)
Re-Aluminizing sequence 1. Wash by water 2. Remove old aluminum by Sodium hydroxide(NaOH) 3. Polish by Sodium Hydrogen Carbonate ( 2NaHCO 3 ) 4. Wipe by cotton cloth with alcohol 5. Install mirror in the Vacuum chamber
6. Pumping vacuum camber into 5X10-6 torr. (Use the cryio-pump & the Meissner-coil pump) 7. Ion-bombardment (3X10-2 torr 20min.) 8. One more Pumping vacuum camber into 5X10-6 torr. (Use the cryio-pump & the Meissner-coil pump) 9. Spatter aluminum (6 times X 6 filaments about 30min.) 10. Take out mirrors from chamber 11. Packing mirror to transportation box.
![Page 11: Re-aluminizing of 60cm mirror at Maidanak Observatory Kiichi Okita*, Takashi Ito**, Fumi Yoshida**, Seitaro Urakawa***, Kenshi Yanagisawa*, Daisuke Kuroda*,](https://reader036.vdocuments.mx/reader036/viewer/2022062421/56649cad5503460f949702fa/html5/thumbnails/11.jpg)
Cryio-pump
Filament for heat-up Aluminum
Meissner-coil LqN2 flow into the copper pipe and Cool down, then trap water vapor in the chamber
At the opposite side that installed mirrors, there are 36 filaments at the wall of the chamber.
![Page 12: Re-aluminizing of 60cm mirror at Maidanak Observatory Kiichi Okita*, Takashi Ito**, Fumi Yoshida**, Seitaro Urakawa***, Kenshi Yanagisawa*, Daisuke Kuroda*,](https://reader036.vdocuments.mx/reader036/viewer/2022062421/56649cad5503460f949702fa/html5/thumbnails/12.jpg)
Re-Aluminizing sequence 1. Wash by water 2. Remove old aluminum by sodium hydroxide(NaOH) 3. Polish by Sodium Hydrogen Carbonate ( 2NaHCO 3 ) 4. Wipe by cotton cloth with alcohol 5. Install mirror in the Vacuum chamber 6. Pumping vacuum camber into 5X10-6 torr. (Use the cryio-pump & the Meissner-coil pump)
7. Ion-bombardment (3X10-2 torr 20min.) 8. One more Pumping vacuum camber into 5X10-6 torr. (Use the cryio-pump & the Meissner-coil pump)
9. Spatter aluminum (6 times X 6 filaments about 30min.) 10. Take out mirrors from chamber 11. Packing mirror to transportation box.
![Page 13: Re-aluminizing of 60cm mirror at Maidanak Observatory Kiichi Okita*, Takashi Ito**, Fumi Yoshida**, Seitaro Urakawa***, Kenshi Yanagisawa*, Daisuke Kuroda*,](https://reader036.vdocuments.mx/reader036/viewer/2022062421/56649cad5503460f949702fa/html5/thumbnails/13.jpg)
Ion-bombardment
Sputter aluminum from heated filament
A window glass of vacuum chamber coated from inside with Aluminum
![Page 14: Re-aluminizing of 60cm mirror at Maidanak Observatory Kiichi Okita*, Takashi Ito**, Fumi Yoshida**, Seitaro Urakawa***, Kenshi Yanagisawa*, Daisuke Kuroda*,](https://reader036.vdocuments.mx/reader036/viewer/2022062421/56649cad5503460f949702fa/html5/thumbnails/14.jpg)
Re-Aluminizing sequence 1. Wash by water 2. Remove old aluminum by Sodium hydroxide(NaOH) 3. Polish by Sodium Hydrogen Carbonate ( 2NaHCO 3 ) 4. Wipe by cotton cloth with alcohol 5. Install mirror in the Vacuum chamber 6. Pumping vacuum camber into 5X10-6 torr. (Use the cryio-pump & the Meissner-coil pump) 7. Ion-bombardment (3X10-2 torr 20min.) 8. One more Pumping vacuum camber into 5X10-6 torr. (Use the cryio-pump & the Meissner-coil pump) 9. Spatter aluminum (6 times X 6 filaments about 30min.)
10. Take out mirrors from chamber 11. Packing mirror to transportation box.
![Page 15: Re-aluminizing of 60cm mirror at Maidanak Observatory Kiichi Okita*, Takashi Ito**, Fumi Yoshida**, Seitaro Urakawa***, Kenshi Yanagisawa*, Daisuke Kuroda*,](https://reader036.vdocuments.mx/reader036/viewer/2022062421/56649cad5503460f949702fa/html5/thumbnails/15.jpg)
After re-aluminizing mirrors. 60cm, 50cm, small mirrors.
60cm main mirror
50cm main mirror
![Page 16: Re-aluminizing of 60cm mirror at Maidanak Observatory Kiichi Okita*, Takashi Ito**, Fumi Yoshida**, Seitaro Urakawa***, Kenshi Yanagisawa*, Daisuke Kuroda*,](https://reader036.vdocuments.mx/reader036/viewer/2022062421/56649cad5503460f949702fa/html5/thumbnails/16.jpg)
Re-Aluminizing sequence 1. Wash by water 2. Remove old aluminum by Sodium hydroxide(NaOH) 3. Polish by Sodium Hydrogen Carbonate ( 2NaHCO 3 ) 4. Wipe by cotton cloth with alcohol 5. Install mirror in the Vacuum chamber 6. Pumping vacuum camber into 5X10-6 torr. (Use the cryio-pump & the Meissner-coil pump) 7. Ion-bombardment (3X10-2 torr 20min.) 8. One more Pumping vacuum camber into 5X10-6 torr. (Use the cryio-pump & the Meissner-coil pump) 9. Spatter aluminum (6 times X 6 filaments about 30min.) 10. Take out mirrors from chamber
11. Packing mirror to transportation box.
![Page 17: Re-aluminizing of 60cm mirror at Maidanak Observatory Kiichi Okita*, Takashi Ito**, Fumi Yoshida**, Seitaro Urakawa***, Kenshi Yanagisawa*, Daisuke Kuroda*,](https://reader036.vdocuments.mx/reader036/viewer/2022062421/56649cad5503460f949702fa/html5/thumbnails/17.jpg)
Pack mirrors in the box 60cm main mirror
50cm main mirror and small mirrors
![Page 18: Re-aluminizing of 60cm mirror at Maidanak Observatory Kiichi Okita*, Takashi Ito**, Fumi Yoshida**, Seitaro Urakawa***, Kenshi Yanagisawa*, Daisuke Kuroda*,](https://reader036.vdocuments.mx/reader036/viewer/2022062421/56649cad5503460f949702fa/html5/thumbnails/18.jpg)
Wyko NT1100 (Veeco co.)Height accuracy <0.3nmMeasurement accuracy about ~ 1nm
Measured 3 times each point
Result : 130nm ~ 140nm
Measurement of thickness 2010.5.13 by S. Ozaki (NAOJ) Preparation plate
(Use 3 plates)
Measurement point
Preparation plate from the side view
Aluminum