NACE CORROSION 2008TEG 096X Symposia - Paper 1421
Electrochemical Studies with Coupled Multielectrode Array Sensors on Corrosion Inhibition of Copper and Affected Metals
in the Presence of Ammonia and Other Corrosive Ions In Zero Liquid Discharge Cooling Water
Dan DukeWater Conservation Technology International, Inc.
Temecula, CA
Lietai YangCorr Instruments, LLC
San Antonio, TX
![Page 2: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/2.jpg)
2
Presentation Outline• Wastewater Reuse in Zero Liquid
Discharge (ZLD) Towers• Corrosion of Copper by Ammonia• Coupled Multielectrode Array Sensor
(CMAS) Corrosion Studies• Municipal Reuse Case History• Galvanized Metal Study
![Page 3: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/3.jpg)
This technology is patent protected;
US 6,929,749 / Silica Scale ControlUS 6,949,193 / Silica Scale ControlUS 6,998,092 / Corrosion Inhibition/SilicaUS 7,122,148 / Corrosion Inhibition/Silica Additional patents are pending
![Page 4: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/4.jpg)
Wastewater Reuse in Zero Liquid Discharge (ZLD) Towers
Silica Inhibition Chemistry
![Page 5: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/5.jpg)
5
Reuse of Wastewater for Cooling Tower Makeup
• Waste water requires treatment to remove suspended solids (TSS) & insoluble organics
• Filtered to remove TSS that would foul softener• Need high efficiency softening (HES)• Dissolved solids (TDS) must be low enough to
permit ion exchange softening• Natural high silica and alkalinity desirable• Ammonia and soluble organics do not have to
be removed with ZLD / silica chemistry
![Page 6: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/6.jpg)
6
Cost Benefits ofZLD Tower Operation
• High efficiency softening lowers salt use (4# per CF resin) and brine waste flow (< 2% MU)
• Typical softening cost of $0.12 per 1000 gallons tower makeup
• Both equipment and operating cost is 10-15% of conventional ZLD / discharge reduction systems
• Optimum water use and discharge reduction• Reduced wastewater discharge obtained with
use of waste heat (low carbon footprint)
![Page 7: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/7.jpg)
7
ZLD / Silica Chemistry Expanded Options
• Permits use of alternative water sources such as municipal / industrial reuse, RO reject, and high TDS water sources for tower makeup
• Silica inhibits metals from corrosion by high TDS (azoles needed for copper / ammonia)
• Expands metal selection / cost economy• Soft water eliminates scale limitations and
permits higher temperatures• Biostatic chemistry mitigates micro-bio activity
![Page 8: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/8.jpg)
Corrosion of Copper by Ammonia
![Page 9: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/9.jpg)
9
Corrosion Rates of Several Copper Alloys in 0.8% Ammonia at 104o F (40o C)
Alloy Corrosion Ratesmpy mm/y
Copper 14 0.30Brass (Cu-Zn, 70:30) 7 0.20Alloy 905 (Cu-Sn-Zn) 5 0.10Cu-Mn (95:5) 2 0.05
Source: Radley, Stanley and Moss, Corrosion Technology 6:229:1959
![Page 10: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/10.jpg)
10
Copper Corrosion Inhibition Study(Azoles in High Ammonia / ZLD Water)
• Study with 150,000 mg/L TDS / pH 10 / soft tower water inhibited by silica and azoles exposed to ammonia (200-400 mg/L)
• Rapid uninhibited corrosion by ammonia• Azoles highly effective for inhibiting ammonia
attack at high pH / TDS• High pH treatment method increases azoles
effectiveness / cost efficiency
![Page 11: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/11.jpg)
11
Copper / TTA / Ammonia Study and Weight Loss Results
ZLD Tower Water NH4+, mg/L TTA, mg/L Cu, mg/L CR, mpyWt. loss
Sample # 1 0 0 0.7
Beginning 300 0 0.7
After 48 hours 300 0 40
Sample # 2 0 0 0.7
Beginning 300 200 0.7
After 48 hours 300 200 0.7
0.0
2.5
Copper Corrosion Inhibition by TTA (Ammonia / pH 10 and 150,000 TDS)
![Page 12: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/12.jpg)
CMAS Corrosion Studies
Localized Corrosive Effects of Ammonia, High TDS, High pH on
Copper Zinc and Aluminum
![Page 13: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/13.jpg)
13
15% NaCl solution with pH adjusted, no Inhibitors, Ammonia / TDS / pH corrosive effect on Cu and Zn
0.01
0.10
1.00
10.00
100.00
1000.00
7/21/07 7/22/07 7/23/07 7/24/07 7/25/07 7/26/07
Date
Max
imum
Rat
e (m
py)
Copper 110Zinc
NaOH added, pH =10 using
pH=8.15 125 ppm ammonia added pH=10.75
![Page 14: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/14.jpg)
14
Silica Inhibited ZLD Water, Zn & Al Inhibited, Cu corroded by Ammonia / TDS / pH
0.01
0.10
1.00
10.00
7/7/07 7/9/07 7/11/07 7/13/07 7/15/07 7/17/07 7/19/07 7/21/07Date
Max
imum
Rat
e (m
py)
Aluminum 1100Copper 110Zinc
125 ppm ammoniaadded
250 ppm ammonia added
![Page 15: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/15.jpg)
15
ZLD (150,000 TDS) / Silica treated Tower Water: Ammonia and TDS Corrosion of Copper inhibited by TTA
0.001
0.010
0.100
1.000
10.000
7/22/07 7/27/07 8/1/07 8/6/07 8/11/07 8/16/07 8/21/07 8/26/07
Date
Max
imum
Rat
e (m
py)
Aluminum 1100Copper 110Zinc
Probes newly polished
125 ppmammoniaadded
375 ppm ammonia added
![Page 16: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/16.jpg)
16
CMAS Study Summary
• Uninhibited localized corrosion rates with ammonia and high TDS were 2.5 mpy for copper and 80 mpy for zinc (room temperature)
• Silica inhibited localized corrosion rates for zinc and aluminum were negligible from ammonia / high TDS; copper was not well inhibited
• Copper was inhibited by TTA to negligible corrosion rate from high ammonia / high TDS
![Page 17: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/17.jpg)
Municipal Reuse Case History
Municipal Reuse water used for makeup to ZLD Tower Operation
![Page 18: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/18.jpg)
18
Cooling Tower Using High Ammonia (Reuse) Waste Water for Makeup
• High ammonia (34 mg/L) “reuse” makeup water• High hardness and phosphates limit traditional COC
(concentrations of chemistry) of makeup in tower• High TDS limited traditional corrosion protection• Copper chiller and absorber tubes at risk from ammonia• Required multimedia filtered and HES softened makeup• ZLD / high pH / high TDS with silica & TTA inhibitors • Ammonia stripped to < 0.5 mg/L at 60 COC by chemistry• Corrosion of copper inhibited to 0.007 mpy.• Micro-bio growth (organics) mitigated (10o Col / ml).
![Page 19: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/19.jpg)
19
Tower Ammonia StrippingIn a waste stream, ammonium ions exist in equilibrium with ammonia.
1. Below pH 7, virtually all the ammonia is soluble ammonia ions.2. Above pH 12, virtually all the ammonia is present as a
dissolved gas.3. Between pH 7 and 12, both ammonium ions and dissolved gas
exist together. 4. Percentage of dissolved gas increases with pH / temperature. 5. Elevated pH and temperature favor removal of ammonia from
solution as the gas when water is scrubbed over a tower.
![Page 20: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/20.jpg)
20
Tower / Soft Makeup COC (Concentration of Chemistry) RatiosSample / Tests (01/04/08) Tower Soft MU COC
TDS, mg/L (Myron L 6P, 442) 66000 1100 60 pH 9.85 7.3 NASilica, mg/L SiO2 530 20 27 Calcium, mg/L CaCO3 18 0.2 NA
Magnesium, mg/L CaCO3 13 0.1 NASulfate, mg/L SO4 7700 128 60 Chloride, mg/L NaCl 12500 212 59 Tot. Alkalinity, mg/L CaCO3 15000 257 58Ammonia, mg/L NH4 < 0.5 38 NATotal Phosphate, mg/L PO4 52 0.9 58TTA, mg/L as tolytriazole 5 NA NA
ZLD Cooling Tower using (California Title 22) Municipal Reuse Waste Water for Makeup
![Page 21: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/21.jpg)
21
Corrosion Rates for ZLD Cooling Tower with Reuse Makeup Water
Linear Polarization and Weight Loss Corrosion Rates(Water treated with silica and TTA inhibitors)
Mild Steel (1008) Copper (110)
Linear Polarization (mpy) 0.2 < 0.1
Coupon Weight Loss with 60 day exposure
(mpy)0.22 0.007
![Page 22: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/22.jpg)
22
Biostatic Monitoring
• Dip stick cultures 10o Col / ml @ 48 hours• No bio slime deposits on tower fill• No slime in chillers or absorbers• No odor• No biocide use or handling
![Page 23: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/23.jpg)
23
Natural Biostatic Chemistry
• Natural source water alkalinity and TDS• Elevated pH and TDS are naturally
biostatic to bacteria, spores and viruses• Hydrolysis of peptide chains as water pH
is increased (used in waste treatment)• Denaturing of proteins or enzymes by
elevated TDS • Report by Anderson Engineering
![Page 24: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/24.jpg)
24
Non-scaling Water Savings
• HES softening provides non-scaling water • Permits high COC or ZLD operation• Water use was reduced 30% (reduced
tower blowdown)• Reuse water cost / HCF was 30% less• Total water use cost reduced 50%• Equipment ROI less than 12 months• Minor chemical use (TTA)
![Page 25: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/25.jpg)
Galvanized Coating Passivation Study
ZLD Cooling Water
![Page 26: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/26.jpg)
26
Tower / Soft Makeup COC (Concentration of Chemistry) Ratios
Sample / Tests Tower FilteredSample Soft MU COC
TDS, mg/L (Myron L 6P) 146,000 251 582pH 10.07 7.58Copper, mg/L Cu 0.7 0.25 0.0015 467Iron, mg/L Fe 22.2 ND NDZinc, mg/L Zn 3.8 ND NDSilica, mg/L SiO2 1,050 30 35Calcium, mg/L CaCO3 62 12.4 <0.1Magnesium, mg/L CaCO3 16 8.2 <0.1Phosphate, mg/L PO4 89 0.15 593Nitrate, mg/L NO3 2590 4.5 575 Sulfate, mg/L SO4 10,260 18 570Chloride, mg/L NaCl 22,400 38 589Tot. Alkalinity, mg/L CaCO3 69,400 120 578
ZLD Tower Water Chemistry
![Page 27: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/27.jpg)
27
Galvanized coupon #283 exposed in ZLD tower for 60 days
vs #282 control before & after coating striped
![Page 28: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/28.jpg)
28
ZLD Chemistry / Passivation of Galvanized Coatings
• Galvanized coatings protected by silica• Not affected by high alkalinity / pH / TDS• Residual copper from source water may
deposit on non-passivate coating• Micro pitting of non-passivate coating• TTA / azoles (25 mg/L active dose) at start
up very effective to passivate coating• Periodic azoles dose for residual copper
![Page 29: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/29.jpg)
29
Galvanized Coupon exposed 60 days in ZLD tower with TTA Supplement to Silica Inhibitor
![Page 30: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/30.jpg)
30
ZLD / Silica / TTA Chemistry Summary
• No scale threat with “ZLD” operation• Negligible corrosion at very high TDS• Unaffected by reuse (ammonia) waste water• Ammonia and organics stripped by chemistry• Copper protected from ammonia• Mitigates biological and pathogen growth• Simple control chemistry• Reduced water use and discharge cost
![Page 31: NACE CORROSION 2008 TEG 096X Symposia - Paper 1421P08372).pdf · NACE CORROSION 2008 TEG 096X Symposia - Paper 1421 Electrochemical Studies with Coupled Multielectrode Array ... •](https://reader030.vdocuments.mx/reader030/viewer/2022011800/5acedec27f8b9a56098c56c1/html5/thumbnails/31.jpg)
31
Questions?