mrs dec 2010 steel with copper precipitates dierk raabe
DESCRIPTION
Copper nanoprecipitates in steel studied by atom probe tomography and ab initio based Monte Carlo simulation Authors: O. Dmitrieva, P.-P. Choi, T. Hickel, N. Tillack, D. Ponge, J. Neugebauer, D. Raabe MRS Fall Meeting 2010TRANSCRIPT
![Page 1: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/1.jpg)
O. Dmitrieva, P.-P. Choi, T. Hickel, N. Tillack, D. Ponge, J. Neugebauer, D. Raabe
Düsseldorf, [email protected]
Thanks to: DFG
MRS Fall Conference 30. November 2010 Dierk Raabe
Copper nanoprecipitates in steel studied by atom probe tomography and ab initio based Monte Carlo simulation
![Page 2: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/2.jpg)
Motivation: Electromobility
Fe-3%Si-1% (2%) Cu model system
Fe-3%Si-Cu engineering alloy
Simulations (DFT + kMC, model system)
Conclusions and challenges
Overview
Raabe: Adv. Mater. 14 (2002), Roters et al. Acta Mater.58 (2010)
![Page 3: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/3.jpg)
3
Avoid use of permanent magnets and use instead electrical magnets in synchronous electrical engines
High strength soft magnetic steels in car engines reduce CO2 emission
www.mpie.de
Motivation
![Page 4: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/4.jpg)
4
Electrical steels for electrical cars
![Page 5: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/5.jpg)
5
Electrical steels
Standard soft magnetic steel: based on
Fe3 wt. % Si
ferritic phase, coarse grains
soft-magnetic properties
Improvement of the mechanical strength!
precipitation hardening: 1-2 wt. % Cu, aging at 450°C
![Page 6: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/6.jpg)
6
Nano-precipitates in soft magnetic Fe-3%Si steels
size Cu precipitates (nm)
{JP 2004 339603}
15 nm
magneti
c lo
ss (
W/k
g)
Fe-Si steel with Cu nano-precipitates
nanoparticles too small for Bloch-wall interaction but effective as dislocation obstacles
mechanically very strong soft magnets for motors
{Jä
nic
he e
t al.,
Werk
stoff
kunde S
tahl}
20 nm
0,2 µm0,1 µm 0,3 µm
![Page 7: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/7.jpg)
Overview
www.mpie.de
Motivation: Electromobility
Fe-3%Si-1% (2%) Cu model system
Fe-3%Si-Cu engineering alloy
Simulations (DFT + kMC, model system)
Conclusions and challenges
![Page 8: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/8.jpg)
8
Precipitation hardened materials
Precipitation hardened electrical steels:
nucleation of copper precipitates in iron-silicon matrix
Fe
Si 3 wt. %
Cu 1 wt. %
Fe
Si 3 wt. %
Cu 2 wt.%
• solute annealing 950°C-1150°C for 1h
• water quenching
• age hardening at 400-450°C for 10 min - 100 h
I. II.
Fe-3wt% Si
Cu
CuCu
www.mpie.de
![Page 9: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/9.jpg)
9
Precipitation hardened electrical steels
Time, min
Atom probe tomography
10 min 120 min 6000 min
www.mpie.de
![Page 10: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/10.jpg)
10
3D Atom Probe Tomography
LEAP (Local Electrode Atom Probe) 3000X HR
3-dimensional reconstructed
model of specimen(about 100 Millions of atoms)
200 nm
initiated evaporationbyor
Time of flight
spatial resolution
layer-by-layer
high voltage 10 kV
+ –
100 nm
48Ti+2
55Mn+2
54Fe+2
56Fe+2 58Ni+2
60Ni+2
24 26 28
time of flight mass / charge state
![Page 11: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/11.jpg)
11
APT results: 3D atomic maps (Laser mode at 60K, 0.4 nJ)
120 min
Cu 1 wt.%
nm
Fe; Cu
nm
Iso-concentration surfaces at Cu 11 at.%www.mpie.de
![Page 12: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/12.jpg)
12
120 min
20 nm
20 nm
6000 min
20 nm
20 nm
120 min 6000 min
Iso-concentration surfaces at Cu 11 at.%
Cu 1 wt.% Cu 2 wt.%
APT results: 3D atomic maps (Laser mode at 60K, 0.4 nJ)
450°C aging
Fe-Si-Cu, LEAP 3000X HR
www.mpie.de
![Page 13: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/13.jpg)
13
APT results: quantification
Cu 1 wt.% Cu 2 wt.%
“Enrichment factor”:
Fe 0.68Cu 40.1Si 0.75
Fe 0.65Cu 44.0Si 0.68
Fe 0.77Cu 17Si 0.78
Fe 0.56Cu 31.9Si 0.58
volume fraction of clusters 2% 2% 5% 3-5%
120 min 6000 min 120 min 6000 min
3.2 nm ± 0.8 nm 5.0 nm ± 0.8 nm 4.3 nm ± 0.8 nm 6.5 nm ± 1.4 nm
Matrix (without clusters):Cu 0.2 at% Cu 0.1 at% Cu 0.2 at% Cu 0.1 at%
Cluster:Fe 62.9 at%Cu 32.1 at%Si 5.0 at%
Cluster:Fe 60.7 at%Cu 35.2 at%Si 4.1 at%
Cluster:Fe 51.8 at%Cu 44.6 at%Si 3.6 at%
Cluster:Fe 71 at%Cu 24 at%Si 5 at%
content in clustercontent in alloy
6.11023 0.91023 6.41023 0.61023
clusters number density, m-3
www.mpie.de
![Page 14: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/14.jpg)
14
APT results: Proximity histogram
20 nm
Cu 2 wt.%; 450°C/6000 min
• kinetic reasons?
(different stages of particle growth)
• slow diffusion; misfit ?
residual Fe-content
diffuse interface
Cluster size5 nm8 nm
bigger cluster
smaller cluster
matrixnm
cluster center
www.mpie.de
![Page 15: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/15.jpg)
Overview
Motivation: Electromobility
Fe-3%Si-1% (2%) Cu model system
Fe-3%Si-Cu engineering alloy
Simulations (DFT + kMC, model system)
Conclusions and challenges
www.mpie.de
![Page 16: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/16.jpg)
16
Overall content in the analysis volume:
Fe 92.1 at.%
Cu 1.49 at.%
Al 0.56 at.%
Si 5.83 at. %
APT results
www.mpie.de
![Page 17: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/17.jpg)
O. Dmitrieva
17
Fe Si 17924-1FB3wt%Si, 2wt%Cu
Iso-concentration-Surfaces at Cu 6 at.%
3D-concentration profiles
www.mpie.de
![Page 18: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/18.jpg)
18
d = 5.0 ± 1.0 nm(density corrected:d = 6.0 ± 1.4 nm)
Cluster analysis
(cluster analysis: Nmin=100,dmax=0.7 nm)
www.mpie.de
![Page 19: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/19.jpg)
Overview
Motivation: Electromobility
Fe-3%Si- 1% (2%) Cu model system
Fe-3%Si-Cu engineering alloy
Simulations (DFT + kMC, model system)
Conclusions and challenges
www.mpie.de
![Page 20: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/20.jpg)
Modeling: ab-initio, DFT / GGA, binding energies
Fe-Si steel with Cu nano-precipitates
![Page 21: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/21.jpg)
Modeling: ab-initio, DFT / GGA, binding energies
Fe-Si steel with Cu nano-precipitates
![Page 22: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/22.jpg)
Modeling: ab-initio, DFT / GGA, binding energies
Fe-Si steel with Cu nano-precipitates
![Page 23: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/23.jpg)
Modeling: ab-initio, DFT / GGA, binding energies
Fe-Si steel with Cu nano-precipitates
![Page 24: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/24.jpg)
24
Ab-initio, binding energies: Cu-Cu in Fe matrix
Fe-Si steel with Cu nano-precipitates
![Page 25: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/25.jpg)
25
Ab-initio, binding energies: Si-Si in Fe matrix
Fe-Si steel with Cu nano-precipitates
![Page 26: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/26.jpg)
26
For neighbor interaction energy take difference (in eV)
(repulsive) = 0.390 (attractive) = -0.124 (attractive) = -0.245
ESiSibin
ESiCubin
E CuCubin
Ab-initio, binding energies
Fe-Si steel with Cu nano-precipitates
![Page 27: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/27.jpg)
27
Ab-initio, use binding energies in kinetic Monte Carlo model
www.mpie.de
![Page 28: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/28.jpg)
Overview
Motivation: Electromobility
Fe-3%Si-1% (2%) Cu model system
Fe-3%Si-Cu engineering alloy
Simulations (DFT + kMC, model system)
Conclusions and challenges
www.mpie.de
![Page 29: MRS Dec 2010 Steel With Copper Precipitates Dierk Raabe](https://reader037.vdocuments.mx/reader037/viewer/2022103018/55893465d8b42a2d398b45be/html5/thumbnails/29.jpg)
29
Conclusions and challenges
Soft magnetic steels for electromobility
Increase mechanical strength without loosing good soft magnetic properties
Use nanoprecipitates with size below Bloch wall thickness
APT suited to provide statistics and composition of nanoparticles
Ab-initio thermodynamics in system Fe-Si-Cu
Kinetics: QM – kMC
Coupling DFT/kMC with atomic-scale experiments
www.mpie.de