Gas Diffusion Barriers Using Atomic Layer Deposition: A New Calcium Test
and Polymer Substrate Effects
by
JACOB ANDREW BERTRAND
B.S., University of Redlands, 2005
A thesis submitted to the
Faculty of the Graduate School of the
University of Colorado in partial fulfillment
of the requirements for the degree of
Doctor of Philosophy
Department of Chemistry
2012
![Page 2: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/2.jpg)
This thesis entitled:
Gas Diffusion Barriers Using Atomic Layer Deposition:
A New Calcium Test and Polymer Substrate Effects
by Jacob Andrew Bertrand
has been approved for the Department of Chemistry
______________________________ Steven M. George
______________________________ Douglas L. Gin
___________________ Date
The final copy of this thesis has been examined by the signatories, and we find
that both the content and the form meet acceptable presentation standards of
scholarly work in the above mentioned discipline.
![Page 3: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/3.jpg)
iii
Bertrand, Jacob Andrew (Ph.D., Chemistry)
Gas Diffusion Barriers Using Atomic Layer Deposition: A New Calcium Test and Polymer Substrate Effects
Thesis directed by Professor Steven M. George
Abstract The increasing demand on available energy resources has led to a desire for
more energy efficient devices. The wide use of displays in consumer electronics, such as
televisions, cell phones, cameras and computers makes them an ideal target for improvement.
Organic light-emitting diodes (OLEDs) are a good candidate to replace traditional Si based
devices. However, the low work function metals typically used as electrodes in OLEDs are very
reactive with water and oxygen. Ultralow permeability gas diffusion barriers with water vapor
transmission rates (WVTRs) as low as <10-6 g/(m2*day) are required on the polymers used to
fabricate organic electronic and thin film photovoltaic devices.
Atomic Layer Deposition (ALD) uses self-limiting surface reactions to deposit thin
conformal films. ALD is capable of depositing thin, conformal, high quality barriers. WVTR
values as low as 5 x 10-5 g/(m2*day) have been measured for Al2O3 ALD films at 38C/85% RH
using the Ca test with optical transmission probing. The Ca test is a technique with very high
sensitivity to measure ultralow WVTRs. This test relies on measuring the oxidation of a Ca
metal film by monitoring the change in its optical or electrical properties. However, glass lid
control experiments have indicated that the WVTRs measured by the Ca test are limited by H2O
permeability through the epoxy seals. Varying results have been reported in the literature
using the electrical conductance of Ca to measure permeation.
![Page 4: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/4.jpg)
iv
In this work, two approaches were applied to overcome the epoxy edge seal limitations.
The first approach was to deposit Al2O3 ALD barriers directly on Ca metal. While the Al2O3 ALD
barriers were successfully deposited, the measurement of an accurate WVTR was limited by
barrier pinholes. The presence of pinholes in the Al2O3 ALD barrier on Ca results in the localized
oxidation of the Ca sensor. Heterogeneous degradation of the Ca causes inaccuracies in the
conductance of the film. As oxidation regions merge, large percolation paths are severed
without complete Ca oxidation. To solve this problem, a new apparatus was developed that
measures the electrical conductance of Ca films. This new apparatus does not rely on epoxy
seals and separates the Ca metal from the barrier. Unfortunately, the electrical conductance of
the Ca film versus Ca oxidation was found to be extremely nonlinear. This nonlinearity severely
complicates the usual analysis to obtain WVTR values from the Ca test.
The new apparatus was useful for the examination of PEN polymer substrates using the
total lifetime of the Ca sensor. Polymer effects on the measurement of gas permeability for
polymer/barrier systems have largely been ignored. Experiments were performed to determine
the effect of the PEN polymer substrates on the WVTR measurement. The H2O permeation
activation energy in the PEN polymer, the effect of water saturation of the PEN polymer and
the dependence of the lifetime of the Ca sensor on the H2O flux on the PEN substrate were of
particular interest. The experiments obtained H2O permeation activation energies in the PEN
polymer of 12.4 kJ/mol. The Ca sensor lifetime was found to be linear with H2O flux. No
difference in Ca sensor lifetime was observed between dry or H2O-saturated PEN polymer
substrates.
![Page 5: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/5.jpg)
Dedication I dedicate this work to my wife, Dr. Jenny M. Demos-Bertrand for her unfailing love and
support before and throughout this work. I also dedicate it to my father, Capt. Lee S. Bertrand,
for his dedication to his family, his example, and his constant encouragement without which I
would not be the man I am.
![Page 6: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/6.jpg)
vi
Acknowledgements Foremost, I would like to acknowledge my Ph.D. advisor and mentor Dr. Steven M.
George. He provided me with the resources, support, guidance and environment that allowed
me to grow as a scientist. I cannot thank him enough his willingness discuss and explore new
ideas.
My work would not have been possible without the knowledge and help provided by all
of the members of the George Group. I would like to specially thank David Goldstein, Andrew
Cavanagh, Arrelaine Dameron, Dragos Seghete, Layton Baker, Stephen Davidson, Beau Burton,
and Jarod McCormick. They were responsible for teaching me how to build, program and run
ALD reactors. Furthermore, many of them acted as sounding boards for my ideas and were
always willing to help refine and prioritize them. Shih-hui Jen has been invaluable for her help
throughout many facets of my graduate studies. Thank you to Daniel Higgs, Tim Schiesswohl,
Jennifer O’Patchen for their help in executing experiments presented in this work.
The members of the group that I have not mentioned have been just as valuable to me
for their contributions to my experience. From my first day as part of the group they have
made me feel at home and always been willing to lend a hand.
Finally I would like to thank Craig Joy, Jim Kastengren, Don David, Ken Smith, Jonathan
Peterson, Wayne Winkler and Dennis Steffey at the CIRES Integrated Instrument Development
Facility. Their ability to turn scribbles on a board into functional instruments has been integral
to this work. Without them much of what is presented here would have remained ideas.
![Page 7: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/7.jpg)
vii
Table of Contents Abstract ........................................................................................................................................................ iii
Dedication ..................................................................................................................................................... v
Acknowledgements ...................................................................................................................................... vi
List of Tables ................................................................................................................................................. x
List of Figures ............................................................................................................................................... xi
Chapter 1 Introduction ................................................................................................................................. 1
Atomic Layer Deposition ........................................................................................................................... 1
Mechanical Testing ................................................................................................................................... 5
Barrier Testing ........................................................................................................................................... 8
Calcium Test ............................................................................................................................................ 11
Ca Test Electrical Theory ..................................................................................................................... 14
Problems with the Ca Test .................................................................................................................. 17
Substrate Effects ..................................................................................................................................... 19
Equipment ............................................................................................................................................... 22
Glove box ............................................................................................................................................ 22
ALD Reactor ......................................................................................................................................... 22
............................................................................................................................................................ 23
PVD Chamber ...................................................................................................................................... 26
Calcium Sensors .................................................................................................................................. 27
Polymer Substrate ............................................................................................................................... 30
Environmental Chamber ..................................................................................................................... 30
Optical Imaging ................................................................................................................................... 31
Chapter 2 Al2O3 Gas Diffusion Barriers Grown Directly on Ca .................................................................... 32
Abstract ................................................................................................................................................... 32
Introduction ............................................................................................................................................ 33
Experimental ........................................................................................................................................... 35
Ca Deposition Using Glove box with Attached PVD Chamber ............................................................ 35
Al2O3 ALD and ALD Reactor ................................................................................................................. 39
Humidity Chamber, Electrical Conductance, and Photographic Measurements ................................... 39
Results ..................................................................................................................................................... 40
Photographic Images .......................................................................................................................... 40
![Page 8: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/8.jpg)
viii
Electrical Conductance ........................................................................................................................ 43
WVTR from Electrical Conductance .................................................................................................... 45
WVTR from Photographic Images ....................................................................................................... 48
Discussion................................................................................................................................................ 53
WVTR Measurements Using the Ca Test ............................................................................................ 53
Nature of Pinhole Defects Observed By Ca Test ................................................................................. 55
Conclusions ............................................................................................................................................. 57
Chapter 3 A New Calcium Test Apparatus .................................................................................................. 59
Abstract ................................................................................................................................................... 59
Introduction ............................................................................................................................................ 59
Problems with the Ca Test .................................................................................................................. 61
Ca Test Electrical Model ...................................................................................................................... 63
Experimental ........................................................................................................................................... 65
Base Plate and Sensor Holder ............................................................................................................. 66
Electrical Ring ...................................................................................................................................... 68
Adapter Plate ...................................................................................................................................... 70
Sample Cover ...................................................................................................................................... 72
Shroud ................................................................................................................................................. 72
Ca Sensor ............................................................................................................................................. 74
Assembly ................................................................................................................................................. 76
Results and Discussion ............................................................................................................................ 78
Chapter 4 Polymer Substrate Effects .......................................................................................................... 81
Abstract ................................................................................................................................................... 81
Introduction ............................................................................................................................................ 81
Electrical Ca Test ................................................................................................................................. 83
Problems with the Ca Test .................................................................................................................. 84
Experimental ........................................................................................................................................... 86
New Ca Test Apparatus ....................................................................................................................... 88
Results and Discussion ............................................................................................................................ 90
Conclusions ........................................................................................................................................... 100
Chapter 5 Mechanical Testing of ALD ZnO ............................................................................................... 101
Abstract ................................................................................................................................................. 101
![Page 9: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/9.jpg)
ix
Introduction .......................................................................................................................................... 101
Experimental ......................................................................................................................................... 105
Four Point Probe ............................................................................................................................... 106
Confocal Microscopy ......................................................................................................................... 106
ZnO Deposition ................................................................................................................................. 106
Strain Application .............................................................................................................................. 107
Results and Discussion .......................................................................................................................... 109
Crack Mapping .................................................................................................................................. 114
Confocal Microscopy ......................................................................................................................... 116
Conclusions ........................................................................................................................................... 120
Chapter 6 Conclusions .............................................................................................................................. 121
Bibliography .............................................................................................................................................. 124
![Page 10: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/10.jpg)
x
List of Tables Table 1.1 Metal Deposition Conditions………………………………………………………………………………………..29
![Page 11: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/11.jpg)
xi
List of Figures Figure 1.1 Barrier Requirements ................................................................................................................... 3
Figure 1.2 Bent Polymer Cross-sectiion ........................................................................................................ 7
Figure 1.3 Flexed ALD Coated Polymer ......................................................................................................... 7
Figure 1.4 HTO Apparatus ........................................................................................................................... 10
Figure 1.5 DuPont Ca Test Diagram ............................................................................................................ 13
Figure 1.6 Electrical Ca Test Diagram .......................................................................................................... 13
Figure 1.7 Water Diffusion Wavefronts for Barriers on Polymers .............................................................. 16
Figure 1.8 Oxidation Wavefront Forms for a Barrier on Ca ........................................................................ 16
Figure 1.9 Barrier on PEN Schematic .......................................................................................................... 21
Figure 1.10 Schematic of apparatus to prepare Ca films comprised of PVD chamber, glove box and
attached ALD reactor. ................................................................................................................................. 23
Figure 1.11 ALD Reactor Schematic (Top View) .......................................................................................... 23
Figure 1.12 QCM Schematic (Side View) ..................................................................................................... 25
Figure 1.13 Sample Photo ........................................................................................................................... 28
Figure 2.1 Top and side views of Ca film on Au/Cr metal electrodes on glass. .......................................... 38
Figure 2.2 Photographic images of Ca films with thickness of ~270 nm coated with Al2O3 ALD barrier
with thickness of 18.7 nm at 70 °C/28% RH: (A) 23.6 hr; (B) 30.6 hr; (C)37.0 hr; and (D) 55.0 hr............. 42
Figure 2.3 Number of circular spots on Ca film versus time for Al2O3 ALD film with thickness of 18.7 nm
at 70 °C/28% RH. The rapid increase or “blooming” in number of circular spots occurs at ~32 hr. ......... 42
Figure 2.4 Conductance versus time for Ca film with thickness of ~270 nm coated with Al2O3 ALD barrier
with thickness of 18.7 nm at 70 °C/28% RH. The locations A, B, C and D correspond with photographic
images in Figure 2.2. ................................................................................................................................... 44
Figure 2.5 WVTR values corresponding with conductance versus time for Ca film with thickness of ~270
nm coated with Al2O3 ALD barrier with thickness of 18.7 nm at 70 °C/28% RH. ...................................... 47
Figure 2.6 High contrast black-and-white images of Ca film with thickness of ~270 nm coated with Al2O3
ALD barrier with thickness of 18.7 nm at 70 °C/28% RH. ........................................................................... 49
Figure 2.7 Comparison between WVTR values obtained from photographic image and electrical
conductance analysis versus time............................................................................................................... 52
Figure 3.1 Base Plate with Sensor Holder (Top View) ................................................................................. 67
Figure 3.2 Electrical Ring (Top View)........................................................................................................... 69
Figure 3.3 Adapter Plate (Top View) ........................................................................................................... 71
Figure 3.4 Sample Cover (Bottom View) ..................................................................................................... 73
Figure 3.5 Shroud (Bottom View) ............................................................................................................... 73
Figure 3.6 Diagram of Ca sensor ................................................................................................................. 75
Figure 3.7 Fully Assembled Ca Test Apparatus ........................................................................................... 77
Figure 3.8 Baseline Conductance Curve for New Apparatus ...................................................................... 79
Figure 4.1 Bare PEN 70 C / 40% RH ............................................................................................................. 91
Figure 4.2 Ca Film Lifetime vs. 1/Flux ......................................................................................................... 93
Figure 4.3 Conductance vs. Time for Bare PEN with Changing Flux ........................................................... 93
Figure 4.4 Sensor Lifetime vs. Temperature at Constant Flux .................................................................... 95
![Page 12: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/12.jpg)
xii
Figure 4.5 ln(1/Sensor Lifetime) vs. 1/Temperature .................................................................................. 95
Figure 4.6 Water Permeation Through Saturated and Dry Polymers ......................................................... 97
Figure 4.7 Sensor Lifetime vs. percent RH for Dry and Saturated PEN ...................................................... 97
Figure 4.8 Conductance vs. Time for Ca Film Exposed to Atmosphere ...................................................... 99
Figure 5.1 Instron Polymer Flexion Adaptor ............................................................................................. 103
Figure 5.2 Polymer Samples in Flexion Adapter ....................................................................................... 108
Figure 5.3 Avg. Apparent Resistivity vs. Percent Strain, 44nm ZnO ......................................................... 111
Figure 5.4 Avg. Apparent Resistivity vs. % Strain, 100 nm ZnO ................................................................ 111
Figure 5.5 Apparent Resistivity vs. % Strain for 132nm ZnO ALD ............................................................. 113
Figure 5.6 Critical Strain vs. Thickness for 4-Point Probe Method ........................................................... 113
Figure 5.7 Four-Point Probe Crack Mapping ............................................................................................. 115
Figure 5.8 Resistivity vs. Position Plotted in 3-D for 132nm ZnO ............................................................. 115
Figure 5.9 CLSM image of ZnO surface ..................................................................................................... 117
Figure 5.10 Crack Density vs. % Strain for 22nm and 44nm ZnO .............................................................. 117
Figure 5.11 CFM and 4-Point Probe comparison ...................................................................................... 119
Figure 5.12 Crack Density vs. Thickness .................................................................................................... 119
![Page 13: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/13.jpg)
1
Chapter 1 Introduction
Atomic Layer Deposition
Atomic Layer Deposition (ALD) is based on two sequential, self-limiting surface reactions
that yield atomic level control of thin film growth.1 Likewise, the self-limiting nature of the
surface chemistry allows ALD to produce extremely conformal films on very high aspect ratio
structure. The reactants are introduced to the surface in a sequential manner with a sufficiently
long purge of carrier gas in between each reactant dose. Binary compounds lend themselves to
this technique easily since the reaction can be split into two half reactions. The most studied of
these materials is aluminum oxide or alumina (Al2O3). Alumina ALD is performed using trimethyl
aluminum (TMA) and water following the scheme below.
(A) AlOH* + Al(CH3)3 → AlOAl(CH3)2* + CH4
(B) AlCH3* + H2O → AlOH* + CH4
The asterisks indicate the surface species.
The first reaction, (A), shows a dose of TMA reacting with a hydroxylated surface
resulting in a methyl terminated surface. After a purge of inert carrier gas, typically nitrogen,
water is dosed into the reaction chamber. This results in a return to a hydroxylated surface as
shown in step (B). This sequence, ABABAB…, is repeated until the desired thickness is reached.
In order for consistent growth per cycle, the doses of each reactant must be kept sufficiently
large so as to saturate the surface and react with as all available surface sites. The repetition of
these AB cycles results in an Al2O3 ALD growth of 1.1-1.2 Å per AB cycle.2, 3 Previous studies
have shown that Al2O3 ALD can be deposited over a very wide temperature range from 36-200
°C. Al2O3 ALD can also be deposited very effectively on a variety of polymers.4
![Page 14: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/14.jpg)
2
Since first developed in the late 1970’s, ALD has come a long way in terms of the
materials that can be deposited with the technique.5-8 As the number of materials available for
deposition with ALD has increased, so have the number of applications. One growing
application is the use of ALD to create transparent diffusion barriers to protect organic light
emitting diodes (OLEDs)9 and other organic electronic devices10, 11 from degradation by water
and oxygen. The most rigorous barrier requirements exist for OLEDs (Figure 1.1)12. For organic
based electronics to reach device lifetimes comparable to their silicon based counterparts
(>10,000 hrs), they require a water vapor transmission rate (WVTR) of <10-6 g/(m2*day) and an
oxygen transmission rate (OTR) at STP of <10-5 cm3/m2/day.13-16 These requirements arise from
the sensitivity of the low work function metals (Ca, Li, Mg, etc.) necessary to get efficient charge
injection into the organic layers of electroluminescent devices.13-15, 17 Current methods to
protect these devices involve encapsulation of the entire device between glass plates. This
leads to a longer device lifetime but is not necessarily suitable for all applications.18 There is
great interest in creating thinner, flexible, electronics based on organic molecules. This is made
possible by creating the devices on a polymer substrate. However, polymers typically have a
WVTR on the order of 10-0.1 g/(m2*day).15 ALD provides an effective solution to this problem
since ALD is capable of coating devices of any geometry with a conformal film of precisely
controlled thickness.
![Page 15: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/15.jpg)
3
Figure 1.1 Barrier Requirements
![Page 16: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/16.jpg)
4
Al2O3 ALD films of ~12nm are capable of providing diffusion barriers with a WVTR (~10-3
g/(m2*day)) that is a great improvement over the polymer substrates themselves.9, 11, 13
However, these barriers do not meet the requirements discussed earlier. The films still possess
some pinhole defects that limit their effectiveness as barriers.14, 16, 19 Making the barrier layer
thicker will lower the probability of having a defect through the entire layer but results in a film
that is more likely to fracture during processing and handling. Inorganic-organic multilayer
structures have been used to overcome this problem. However, they do not show the decrease
in permeability expected from standard laminate theory, where the total permeation rate can
be obtained by addition of the reciprocals of the permeation rates for each layer (Equation 1).14,
20
( )
Multilayer barriers were first introduced in 1994 and were created using layers of
aluminum metal and acrylate polymer.14 The polymer interlayer provides flexibility as well as
decoupling of defects in the metal or oxide films. This increases the path length of permeants
through the material and decreases the permeation rate for the multilayer14, 16. Multilayer
structures occur in nature and have been shown to the capable of creating extraordinarily
mechanically robust super lattices based on inorganic platelets separated by a polymer
interlayer.21, 22
Multi layering of inorganic and organic materials can be problematic. There can be low
adhesion23 between the layers and decreasing flexibility with increasing thicknesses of
individual layers or the total film.12 Low adhesion can be addressed through the use of
![Page 17: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/17.jpg)
5
molecular layer deposition (MLD). Recent work within our group has shown that it is possible to
deposit polymers using MLD.24, 25 This technique uses the same sequential approach as
described for ALD but deposits an organic molecular fragment during one or both of the steps
in the reaction cycle. One class of materials that can be deposited in this manner is
poly(aluminum alkoxides) or alucones which will be discussed briefly later.26 The precursors
used in MLD are compatible with those used to deposit inorganic materials with ALD which
should lead to good adhesion between the layers. The level of control provided by ALD and
MLD techniques also makes it possible to create graded interfaces between the layers to
increase adhesion. Little has been done to explore the mechanical properties of these
barriers.9, 12 If they are to maintain their integrity while in use on flexible devices, then more
work is needed to understand the behavior of multilayer barriers during flexing. The
mechanical characteristics of the individual layers are particularly important.
Mechanical Testing When a material is flexed, the surface farthest from the center of curvature is put into
tensile strain and the inner surface undergoes compressive strain (Figure 1.3 and Figure 1.2).27
This results in the formation of a neutral plane within the material. If the material is uniform,
i.e. an uncoated polymer, the neutral plane exists in the center of the material. As coatings are
applied, the neutral plane moves away from the center of curvature. In the case of ALD films,
the coatings are three orders of magnitude thinner and the neutral plane remains relatively
unchanged. Linear tensile strain is described by
, where L is the samples original length.
Due to the gradient that exists when a sample undergoes a bending, the strain is obtained
through
, where y is the distance from the neutral plane and R is the radius of
![Page 18: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/18.jpg)
6
curvature.12 The strain at the surface of the substrate is taken to be the strain through the ALD
coating since any gradient that exists within the coating would be negligible. This relationship
leads to the strain applied to an ALD film being
, hs being the thickness of the
substrate.27
As a coated sample is bent, the strain continues to increase until such point that the
coating will fracture. The strain at which this occurs is known as the critical strain (εc) and is
proportional to the reciprocal square root of the film thickness. Initial cracks will lengthen and
additional fractures will occur if the increase in strain continues until the number of fractures
reaches saturation.28 The failure mechanism for thin brittle layers is different from that of bulk
materials. In bulk materials, a crack, once initiated, will propagate the full width across the
material. For thin films, cracks initiate at point defects and propagate to a finite length for a
given strain. As strain increases, the crack length will increase proportionally until either the
maximum stable crack length ( ) or critical crack propagation strain ( ) is reached. Once one
of these conditions is met the crack will propagate to the full width of the film.29
![Page 19: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/19.jpg)
7
Figure 1.3 Flexed ALD Coated Polymer
Figure 1.2 Bent Polymer Cross-sectiion
![Page 20: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/20.jpg)
8
In order to explore these properties of a thin film it is necessary to have a sensitive
technique to monitor changes in the film’s behavior. The changes that occur in film may,
initially, be very small in comparison to the original film. To determine an accurate
measurement of the critical strain, we must be able to detect these minute changes as soon as
they occur during testing. Depending on the properties of the film, i.e. conductivity, there are
few methods that can be used. Indium tin oxide (ITO) is the most studied thin film. As a
conducting oxide it is easily monitored with sensitive resistance measurements.27, 30, 31 Typical
diffusion barriers, are not conducting oxides (Al2O3) and are not capable of such
characterization.
Zinc oxide ALD provides us with a useful analog to explore the mechanical properties
since it is a conductive film. A four-point probe can be used to determine a critical strain. We
can then compare the accuracy of other methods that can be used on non-conductive films.
Barrier Testing Atomic Layer Deposition (ALD) has shown promise as a technique to deposit conformal,
transparent gas diffusion barriers .9, 13 These barriers can protect organic electronic or thin film
solar cell devices from degradation by water and oxygen.10 For organic based electronics to
reach device lifetimes of 10,000 hrs, they require a water vapor transmission rate (WVTR) of
<10-6 g/(m2*day)and an oxygen transmission rate (OTR) at STP of <10-5 cm3/m2/day.15 These
requirements arise from the sensitivity of the low work function metals (e.g. Ca, Li, Mg) in these
devices. There is great interest in fabricating organic electronic devices on flexible polymer
substrates. However, these polymer substrates require a gas diffusion barrier because they
typically have a WVTR on the order of 10-0.1 g/(m2*day).15
![Page 21: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/21.jpg)
9
The development of gas diffusion barriers requires an accurate method for determining
H2O and O2 permeation rates. The only commercial systems available for WVTR measurement
are produced by MOCON.9 Their detection limit of ~10-3 g/(m2*day) is insufficient for testing
ultra-barriers deposited with ALD. In response to this lack of characterization methods, two
primary techniques have been developed to characterize ultra-low steady state permeation
through barriers: the “calcium test” and “HTO tracer method”.9, 13
The HTO tracer method involves placing the films in the apparatus shown in Figure 1.4. A
small amount of 1mCi/g HTO is placed in the vessel base. The barrier coated polymer sample is
enclosed within the vessel with rubber O-rings and a vial containing LiCl is suspended from the
vessels cap. As HTO permeates the polymer/barrier it is absorbed by the hygroscopic salt.
Once the salt vial is removed it is dissolved in a small amount of ultrapure water and a
scintillation cocktail is added. The salt vials are changed roughly every twenty-four hours for
the period of the test, usually 200-300 hours. The results from the scintillation counter can
then be used to determine the WVTR through the sample.9 The downside to this is that only
measurement of the tritium concentration is measured. The assumption is that the tritium
concentration is representative of the water concentration. However, there is evidence that
atomic tritium can diffuse through the barrier with the aid of a proton exchange reaction,
leading an over estimate in the WVTR.32
![Page 22: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/22.jpg)
10
Figure 1.4 HTO Apparatus
![Page 23: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/23.jpg)
11
Calcium Test The calcium test uses a thin, metallic, calcium layer as a sensor for water and oxygen
permeation.9, 12, 13, 16 There are two versions of the Calcium test, both of which rely on
measuring the oxidation of Ca metal.33, 34 The main difference in the methods is how the Ca
oxidation is measured. As oxygen or water permeate the barrier, they react with Ca to form
calcium oxide [CaO] or calcium hydroxide [Ca(OH)2], both of which are transparent to visible
light and electrically insulating
In 2001, Nisato et. al described a testing method using calcium (Ca) metal for measuring
low H2O and O2 permeation rates.33 Their tests relied on using optical observations of the
oxidation of metallic Ca to Ca(OH)2 and CaO to determine calcium corrosion rates. A CCD
camera was used to monitor the reflection from Ca pad. From the images obtained they
measured the area growth of local oxidation regions. Once the growth rate of these areas
becomes linear they use that rate to determine WVTR. These measurements allow the
calculation of the overall degradation rate of the calcium layer and the permeation rate for the
barrier. The WVTR and OTR cannot be easily separated by this method. Further small error is
introduced by the difference in optical constants between the CaO and Ca(OH)2 products.
However, this method is useful to get a baseline measurement of the barrier performance. .
The % transmittance of the sample can also be followed as a function of time. However, the
development of localized oxidation regions will result in sudden increases in the transmittance.
The non-uniformity of the Ca degradation can lead to errors in the determination of a WVTR.
Other groups have subsequently employed the Ca test with optical transmission
probing to measure gas diffusion barriers.35 A similar Ca test method was recently used by
![Page 24: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/24.jpg)
12
DuPont to evaluate Al2O3 ALD barriers on polymer substrates.13 An illustration of the Ca test at
DuPont is shown in Figure 1.5.13 The barrier film is adhered to the Ca test films on a glass
substrate using an epoxy seal. The Ca test revealed that the Al2O3 ALD film was an excellent
barrier and WVTR values less than 5 x10-5 g/(m2*day) were obtained at 38 °C/85% relative
humidity (RH).36
A second implementation of the Ca test has also been developed that relies on
measuring the electrical conductance of a Ca film during oxidation.34 Other groups have also
employed electrical conductance to monitor Ca oxidation.37 In this version of the Ca test,
samples can be prepared by depositing Ca metal on a polymer substrate. A schematic of a
possible experimental configuration adapted from Ref. 34 is shown in Figure 1.6. Silver contacts
were evaporated and the sample was covered with a glass lid using an epoxy seal.
![Page 25: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/25.jpg)
13
Figure 1.5 DuPont Ca Test Diagram
Figure 1.6 Electrical Ca Test Diagram
![Page 26: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/26.jpg)
14
Ca Test Electrical Theory
We will be using the equation originally published by Paetzold in 2003 with some of our own
modifications. The original equation is:
( ) ( )
( )
( )⁄
P = Permeation Rate (g/(m2*day)); n = stoichiometric coefficient; M(Ca) = Molar mass of Ca; M(reagent) = Molar mass of H2O or
O2; δ = density of Ca; ρ = resistivity of Ca; l = separation of contacts; b = width of Ca pad; 1/R = Conductance (mho)
This model makes a few critical assumptions. First, that Ca corrosion is uniform in one
dimension, perpendicular to the barrier. Secondly, that all corrosion is due to either water or
oxygen. Third, the film is uniform in density and resistivity. The fourth and final assumption is
that the area of the Ca pad and the area of the barrier are equal.
If we examine these assumptions we find a few problems. At first it seems reasonable
that, if the barrier is pinhole free, oxidants permeating the barrier will uniformly diffuse.
Barrier permeation is known to be defect-dominated.14, 33 If the barrier is oriented toward the
humid atmosphere the following happens. The oxidant permeates a pinhole and enters the
polymer; the concentration of water expands in all directions equally. This forms a
hemispherical wave that diffuses through the polymer (Figure 1.7). If the separation between
the defects is less than the polymer thickness the hemispheres will join. Once the hemispheres
join, a uniform wave front of water is formed. When this wave front reaches the Ca we would
expect it to also oxidize uniformly. For this to happen all of the defects must have a separation
less than the thickness. The model doesn’t hold true when barrier defects act as point sources.
![Page 27: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/27.jpg)
15
If the defects have very large separations the hemispheres will reach the Ca at individual points.
The Ca will begin to oxidize at a point. The oxidation will spread in a hemispherical wave front
through the Ca just at is did through the polymer. When the Ca film is directly on the barrier,
point sources all that is available for water penetration. Once the oxidation hemisphere has
moved to through the calcium thickness the oxidation will expand in as a cylinder centered on
the defect (Figure 1.8). As oxidation progresses the edges of the cylinders will meet. Depending
on the distribution of defects, large conduction paths can become electrically isolated without
oxidizing all of the Ca metal in the electrical path. Such situations result in a sharp decrease in
conductance resulting from the restricted percolation path rather than true Ca oxidation. This
makes it impossible to determine a WVTR using the standard interpretation of Ca test
conductance curves.
If the barrier is facing the atmosphere this could take days depending on the defect size
and separation. With the barriers facing the Ca sensor, polymer saturation should happen
within a day or two depending on experimental conditions and polymer substrate. Water
absorption by the polymer may lead to barrier disruption if the polymer expands.
The assumption of water being the major oxidant is made because limited results have
shown that the oxidation of the Ca varies greatly with temperature and humidity content. This
has led many to believe that water is the predominant penetrant. This may simply be that the
activation energy need for oxygen to react with a Ca surface is higher than H2O. No apparatus
has yet been built that can separate OTR and WVTR for barrier films. We did not perform these
![Page 28: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/28.jpg)
16
Figure 1.7 Water Diffusion Wavefronts for Barriers on Polymers
Figure 1.8 Oxidation Wavefront Forms for a Barrier on Ca
![Page 29: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/29.jpg)
17
experiments, but our apparatus could be easily adapted to. For the purposes of our work we
will be report the apparent WVTR for barrier films.
Problems with the Ca Test
There are some limitations of the optical implementation of the Ca test. In particular,
the optical Ca test is limited by the epoxy edge seal that provides a path for H2O and O2
diffusion. Recent tests have revealed that Al2O3 ALD barriers on PEN were equivalent to the
glass lid control with using optical Ca test.36 The measured water vapor transmission rate
(WVTR) for both the Al2O3 ALD film and the glass lid yielded effective WVTR values of ~1x10-4
g/(m2*day). This WVTR value was assigned to H2O permeation through the epoxy edge seal.36
With such a high baseline WVTR value, the Ca test cannot easily be used evaluate high quality,
low permeability barriers with a WVTR values at or below 5x10-5 g/(m2*day) at 38 °C/85% RH.
The largest limiting factor for the electrical Ca test is also the epoxy edge seal.
There are other problems with the Ca test using either the optical and conductance
methods. In addition to the epoxy edge sealing, another issue that affects the optical method is
the required modeling of the optical multilayer stack. The modeling is difficult because of a lack
of knowledge regarding the identity of the oxidized Ca sample. The oxidized Ca could be either
CaO or Ca(OH)2 and their optical constants are not known exactly. An unknown, changing,
mixture of the two, which will vary through the test, further complicates attempting the
modeling. This variance is caused by the reaction sequence that Ca metal undergoes when
exposed to water and oxygen. If Ca metal is exposed to oxygen first, it will form CaO (ΔHfo=-
635.09 kJ/mol). If the CaO is sequentially exposed to H2O will with form Ca(OH)2 (ΔHfo=-
986.09). Since only the first change from metal to oxide (or hydroxide) causes a conductance
![Page 30: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/30.jpg)
18
change this means the two permeation rates cannot be separated. The typical solution to this
is that all oxidation is assumed to be due to water permeation and an “effective WVTR” is
typically reported. The optical method suffers further from multiple optical layers with varying
properties that are not known accurately. These layers include the glass substrate, the epoxy,
and the polymer. In addition, the gluing of the polymer to the Ca film on the glass substrate
using epoxy means that the polymer cannot be reused after the Ca test. Consequently, many
individual samples are required to obtain meaningful results.
Other difficulties also affect the Ca test using the conductance method. The
conductance test assumes that uniform Ca oxidation occurs in a top-to-bottom fashion. 34 Since
barrier permeation is known to be defect-dominated, uniform Ca oxidation may not be
occurring if the Ca film is located close to the barrier.14, 38, 39 This is the original configuration
that has been widely used. In the case of pinhole defects, the Ca film may be oxidizing in
localized areas under the pinhole defects. Depending on the distribution of defects, large
conduction paths can become electrically isolated without oxidizing all of the Ca metal in the
electrical path. Such situations result in a sharp decrease in conductance resulting from the
restricted percolation path rather than true Ca oxidation. Oxidation via pinholes occurs in a
hemispherical fashion. As long as the radius of the hemisphere is smaller than the thickness of
the Ca film the electrical method provides a meaningful result.
A second problem for the conductance method arises from the metal used to form the
electrical contacts with the Ca metal. Silver and gold are common choices for good electrical
contacts that will not corrode. Unfortunately, both of these metals form crystalline alloys with
![Page 31: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/31.jpg)
19
Ca at temperatures where the permeation tests are conducted.40, 41 There are multiple alloy
phases that can form, all of which have exothermic enthalpies of formation ranging from -41 to
-106 KJ/mol.42 These alloys are typically studied at elevated temperatures. However, recent
results have shown that annealing at low temperature (270 °C) for as little as 15 minutes can
affect Au-Ca alloy structure.43 This alloy formation leads to changes in the conductance
measurement that cannot be accounted for and increases the uncertainty in the
measurements. Other metals besides silver and gold must be employed to avoid this difficulty.
After noticing this problem with gold contacts we determined that Cr metal made an
appropriate electrical contact.
Substrate Effects Measurements of WVTRs usually ignore the effect of the polymer substrate because the
WVTR of the polymer is so large at ~1 g/(m2*day). Any saturation behavior or lag times
resulting from the polymer substrate are usually assumed to be negligible. However, the
polymer accounts for a significant fraction of the barrier/polymer system. A typical Al2O3 ALD
barrier is 0.025 µm. A typical PEN polymer thickness is 50-200 µm. In addition, the ALD barrier
is usually deposited on only one side of the polymer. As a result of this asymmetry, the ALD
barrier can either face the incident H2O flux or face away from the incident H2O flux. Figure 1.9
shows a representative schematic of an Al2O3 ALD barrier on a PEN substrate. The response to
water exposure by the polymer can have multiple effects on a barrier. Swelling could disrupt a
barrier by applying tensile strain. An accumulation of water at the interface may cause
degradation or delamination of the barrier.
![Page 32: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/32.jpg)
20
One parameter that is often ignored when measuring WVTRs using the Ca test is the
time for the water flux to saturate the polymer. This saturation time is required before H2O can
diffuse through the polymer at a steady state. This time will be included in the barrier’s
measured lag time by the Ca test. The saturation time will depend critically on whether the
ALD barrier faces the incident H2O flux or faces away from the incident H2O flux. If the water
flux is meeting the barrier first the flux into the polymer will be greatly limited. This will
increase the time it takes to fill any bulk reservoir sites in the polymer. The total lag time is the
sum of the time to saturate the polymer and reach steady state diffusion through the barrier.
To understand the times required to saturate the polymer, Ca tests were performed for the
PEN polymer without any ALD barrier. Additional Ca tests were conducted at different
temperatures under constant H2O flux to determine the activation barrier for H2O transport
through the PEN polymer. Further tests were carried out with unsaturated and saturated PEN
to determine the effect of polymer uptake on Ca test performance. After fully understanding
the role of the PEN polymer, we can then return to the ALD barriers on the PEN polymers and
extract meaningful WVTR values. Detailed understanding of the polymer/barrier system should
increase our ability to model such systems.
![Page 33: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/33.jpg)
21
Figure 1.9 Barrier on PEN Schematic
![Page 34: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/34.jpg)
22
Equipment To perform all aspects of this work within our laboratory, an apparatus was built
consisting of a physical vapor deposition (PVD) chamber, a N2 glove box and an attached ALD
reactor. This apparatus is shown in Figure 1.1. An environmental chamber, digital multi-meter
(DMM), USB microscope and computer were also used.
Glove box
A Vacuum Atmospheres Company single workstation Omni-lab glove box was chosen as
the base for our combination system. In order to couple the ALD reactor to the base of the
glove box it was necessary to have a custom attachment ring welded into the bottom of the box
by the manufacturer. The attachment ring was custom manufactured for us by the CIRES
machine shop at the University of Colorado and shipped to the manufacturer. The ring
provides a sealable attachment point for the custom built top flange of the ALD reactor body.
Further modification was made to the right panel of the glove box up receipt. A conflat half
nipple was welded into the side panel to provide an attachment/inlet for the PVD transfer arm.
ALD Reactor
The Al2O3 ALD films were deposited using a low vacuum, hot-wall, viscous flow reactor.
The reactor body consists of a custom reducing cross with a 6” inch body, 3-3/8” CF inlet port
and 2-3/4” CF exhaust port. The body of the reactor in oriented vertically with a custom 8” CF
attached to the glove box. The top is sealed with a hinged lid, providing access to the reactor
chamber. The bottom is a standard CF cap. A conical reducer, 3-3/8” to 2-3/4”, is located on
the inlet side as a small expansion zone. The reducer is capped with a 2-3/4” cap with three ¼”
VCR ports. These ports provide the attachment points for two reactant lines and one high
temperature precursor line.
![Page 35: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/35.jpg)
23
Figure 1.10 Schematic of apparatus to prepare Ca films comprised of PVD chamber, glove box and attached ALD reactor.
Figure 1.11 ALD Reactor Schematic (Top View)
![Page 36: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/36.jpg)
24
One reactant line is dedicated to metal-organic precursors; the other is dedicated to
oxidants. This helps to prevent unwanted deposition in the lines. This decreases particle
generation and maintenance down time. The reactant lines are constantly purged by 100 sccm
of ultrahigh purity (UHP) N2 that is split from a single mass flow controller (MFC).
The reactants for Al2O3 ALD were trimethylaluminum (TMA, Al(CH3)3) and water (H2O).
The reactants were alternately injected into the UHP N2 viscous flow carrier gas continuously
traveling through the reactor (Figure 1.11). The baseline chamber pressure was 1000 mTorr
with the N2 flowing through the reactor. Using computer-controlled pneumatic valves, the
substrate is first exposed to TMA. Subsequently, after N2 purging to remove residual reactants
and reaction products, the substrate is exposed to water and a second N2 purging process. This
sequence defines on AB cycle for Al2O3 ALD. The timing for this sequence was (t1, t2, t3, t4)
where t1 is the TMA exposure time, t2 is the N2 purging time, t3 is the water exposure time and
t4 is the second N2 purging time. The timing sequence was (1, 120, 0.5, 120) where the time are
in seconds. The reactant pressures were both 300 mTorr.
The Al2O3 ALD films were grown to the desired thicknesses by repeating the sequence
for various numbers of AB cycles. The desired Al2O3 ALD barrier were then all deposited at
120-125 °C using trimethylaluminum (Al(CH3)3) and H2O.2, 3 Al2O3 ALD films were deposited on
Ca target directly and on HSPEN (DuPont Teijin Inc.) with a thickness of 200 m depending on
the experiment.
A quartz crystal microbalance (QCM) is a very effective tool for measuring reactant
adsorption and identifying the growth rate.44, 45 The QCM measures the change in vibration
![Page 37: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/37.jpg)
25
Figure 1.12 QCM Schematic (Side View)
![Page 38: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/38.jpg)
26
frequency of a quartz crystal as mass is added to its surface. The change frequency is converted
into a mass per unit area by a thin film deposition monitor. The QCM is used in-situ in an ALD
reactor to detect mass changes per reactant exposure. The technique is sensitive but is limited
because the frequency of the crystal is affected by temperature as well as mass changes.
Consequently maintaining a constant temperature within the reactor is critical. This is
accomplished using computerized feedback controllers for the heaters. The measured mass
can also be affected by unwanted deposition on the “backside” of the crystal. This effect is
countered by carefully sealing the crystal holder to the QCM housing with a conductive epoxy
and a small N2 purge (Figure 1.12). Once saturation conditions for a given chemistry within a
reactor system are determined a QCM is not necessary for every deposition. When not using a
QCM for each deposition the use of a witness wafer is advisable. A witness wafer is a 1” x 1”
square of polished silicon wafer that is placed in the reactor during deposition. After the
reaction is complete the wafer can measured ex-situ to confirm the ALD layer’s thickness,
roughness and density.
A Bede D1 x-ray diffractometer using the Cu Kα (1.71 Å) line was used to measure
witness wafers for this work. Bede REFS fitting software was used to model the obtained
reflectance spectra.
PVD Chamber
The PVD chamber body is a 10” CF cube with ports for pressure measurement, gas
inlets, pumping, the transfer arm and a viewport. The RF source is an Advanced Energy RFX-
600 with an ATX-600 tuning network powering a Kurt J. Lesker Torus magnetron sputter gun.
The chamber is pumped with a Pfeifer turbo pump backed by an oil filled rotary pump. During
![Page 39: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/39.jpg)
27
sputtering the chamber is back filled with Argon (Ar) to the desired pressure. All samples are
spun during deposition using a stepper more to even out inconsistencies.
Calcium Sensors
The Ca sensor is made by starting with a 3” x 1” glass slide. The slides are base bathed
to remove any oils. After removal from the bath they are washed with water, acetone and
methanol. They are left in a methanol bath and placed under a HEPA particle hood. Once
under the hood they are blown dry with filtered N2. Double sided tape is used to attach
stainless steel masks to the glass slides. The masks cover a 0.5” strip down the center of the
glass slide, leaving a 0.25” section on either side to be coated with Chromium (Cr) metal.
Double sided tape is then used to attach multiple masked slides to a sample platter. The slides
are placed inside the PVD chamber and pumped down. Chromium metal is deposited using 400
watts with 15 mTorr partial pressure of Ar for ten minutes (Table 1.1). This gives a contact
thickness of approximately 270 nm. Once deposition is complete the slides are removed and
unmasked. They are visually inspected for contact uniformity; any slides with defects are
discarded. The coated slides are washed with acetone and methanol to remove adhesive
residue. After being blown dry they are cut into three 1”x1” squares. The newly made sensor
substrates are put into the glove box for the next steps. Immediately prior to each test run a
sensor substrate is placed onto a custom PVD sample platter and masked. The mask leaves a
0.75” by 0.5” area for Ca deposition. Care must be taken to ensure that the correct substrate
side is exposed. The platter is inserted into the PVD chamber via the transfer arm and gate
valve. Calcium pads were deposited using the conditions listed in Table 1.1. The samples were
![Page 40: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/40.jpg)
28
Figure 1.13 Sample Photo
![Page 41: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/41.jpg)
29
then returned into the N2 glove box. From there the samples could be directly placed into the
ALD reactor or assembled into the Calcium test apparatus.
In our early experiments Cr/Au contacts were used. Chromium was put down first to
provide an adhesion layer for the subsequent Au. We believed that Au would provide the best
inert and highly contact for the Ca. We observed a change in contact appearance when the
samples were removed from the humidity chamber. When the Ca was first deposited they Ca-
Au contact area appeared smooth to the eye. After being placed the in environmental chamber
they would begin to change to a more crystalline appearance with many facets. An example
photo of one sample is shown in Figure 1.13. Upon investigation we found that Au and Ca form
alloys, even at relatively low temperatures.40, 41 Since Ca and Cu also alloy, albeit at higher
temperatures, we decided to use Cr as our contacts.
Calcium substrates can be re-used after being rinsed in a dilute H2SO4 solution and
cleaned using the initial procedure. This reduces the cost of maintaining the apparatus. Before
reuse the contacts should be inspected for scratches. Good even contacts are very important
for this test.
Table 1.1 Metal Deposition Conditions
Metal Forward Power (watts)
Sample-Target Distance (mm)
Rotational Speed Ar Pressure (mTorr)
Time (min)
Au 300 35 5 15 10
Cr 400 35 5 15 10
Ca 300 35 5 15 10 or 20
![Page 42: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/42.jpg)
30
Polymer Substrate
For this study heat stabilized polyethyl naphthalate (HSPEN) from DuPont Teijin Films,
Q65F, was used as the barrier substrate. PEN is the current substrate of choice for OLED
applications. It has good optical clarity, stability, and smoothness. The heat stabilization process
give the PEN good dimensionally stability when thermally cycled. This is an important property
for a barrier substrate. Thermal cycling applies stress and strain to the ALD barrier.46 This can
lead to delamination and/or fracturing resulting in barrier failure. If the application does not
require optical clarity, heat stability is a key factor in choosing a suitable substrate.
Environmental Chamber
Two humidity chambers were used in this work. The first, for the initial phase, consisted
of an oven containing a saturated salt solution to set the relative humidity within the oven.
This method of setting relative humidity is widely used to calibrate humidity sensors.47, 48 The
standard solution was saturated with MgCl2 to set the oven at ~28%. This solution was chosen
because it was well below 70% RH. This is the humidity at which Al2O3 begins to degrade. The
oven also had a feed through and a viewport, allowing electrical leads and the USB microscope
to monitor the test.
The second chamber was an ESPEC BTL-400 with a heated window and optional side
ports. An in house written Labview program was used to interface with the chambers Watlow
F4 controller. This allowed the conditions within the chamber to be monitored and recorded.
The temperature and humidity ranges are -20 to 180 °C and 10 to 90% RH respectively. These
ranges are well within the capabilities of the Ca test apparatus.
![Page 43: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/43.jpg)
31
Optical Imaging
For the oven/salt solution apparatus a USB microscope was positioned at the oven
viewport to monitor the sample visually. A waterproof USB camera was used with auxiliary
lighting inside the BTL-400 chamber. Image capture software, Flix by Nimisis, was used to
record a sample image every five minutes for the duration of the sample test. These images
were used in order to determine a WVTR that will be described later. The software was also
used to compress the photos into a video to provide a time lapse video of the sample. This
video has proved valuable in evaluating the evolution of sample oxidation. It was these videos
that allowed us to see that there were initial defects, most likely due to particle contamination,
and a bloom of defects, most likely due to defects in the ALD barrier itself.
![Page 44: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/44.jpg)
32
Chapter 2 Al2O3 Gas Diffusion Barriers Grown Directly on Ca
Abstract Al2O3 gas diffusion barriers grown directly on Ca films using atomic layer deposition
(ALD) techniques were evaluated using several methods based on Ca oxidation. The Al2O3 ALD
films were grown on Ca films at 120°C using trimethylaluminum and H2O as the reactants. The
oxidation of the Ca films was then monitored versus time at 70°C and ~28% relative humidity
either by measuring the electrical conductance of the Ca film or by recording the photographic
image of the Ca film. In the photographic images, the Ca films revealed that the Al2O3 ALD films
have a small number of pinhole defects that lead to Ca film oxidation areas that grow radially
around the pinhole defect versus time. A burst of new oxidation areas also appeared suddenly
at later times and grew radially versus time. This rapid “blooming” may be related to another
type of defect caused by water corrosion of the Al2O3 ALD films. In the electrical conductance
measurements, the conductance of the Ca film initially showed little change versus time. The
conductance then dropped rapidly when the oxidation area in the photographic image was a
noticeable fraction of the Ca film area. The conductance measurements yielded a WVTR value
of ~2 x 10-2 g/m2/day prior to the rapid reduction of the conductance. The photographic images
of the Ca film were also analyzed to obtain a WVTR value assuming radial oxidation of the Ca
film around defects. The WVTR values obtained from the electrical conductance and the
photographic images were in approximate agreement and increased versus Ca film oxidation
until the rapid “blooming” of new circular oxidation areas. The WVTR value was also estimated
from the time required for the electrical conductance to be reduced to nearly zero. This
estimated WVTR value of ~0.2 g/m2/day was comparable with the largest WVTR values
![Page 45: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/45.jpg)
33
obtained from the electrical conductance and the photographic images after the onset of the
“blooming”. This study reveals that a range of WVTR values can be obtained from different
variations of the Ca test. There is also a dependence of the WVTR values on the extent of Ca
film oxidation.
Introduction Ultralow water vapor transmission rates (WVTRs) are required for the operation of
organic electronic and thin film photovoltaic devices.49, 50 A WVTR of <10-6 g/m2/day and an
oxygen transmission rate (OTR) at STP of <10-5 cm3/m2/day are needed for organic based
electronics to reach device lifetimes of 10,000 hrs.15, 50 These requirements arise from the
sensitivity of the low work function metals in these devices. Many thin film solar devices also
need WVTR values between 1 x 10-4 and 1 x 10-6 g/m2/day.49 For flexibility, organic electronic
and thin film solar devices could be fabricated on flexible polymer substrates. However,
polymer substrates typically have WVTRs in the range of 10-0.1 g/m2/day and require gas
diffusion barriers to obtain ultralow WVTR values.15
No commercial instrumentation is available to measure ultralow WVTRs. The best
currently available commercial capability is the MOCON Aquatron Model 1 instrument that has
a sensitivity down to WVTR ~ 5 x10-4 g/m2/day (MOCON, Minneapolis, MN). The so-called “Ca
test” using the oxidation of Ca films is one approach that has been employed to measure
ultralow WVTRs. The Ca test can be used in several adaptations. The most widely utilized
methods are based on the electrical conductance of the Ca film,34 the optical transmittance
through the Ca film,51or the oxidized area of the Ca film.16 Other methods that have been
![Page 46: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/46.jpg)
34
developed to measure ultralow WVTRs are based on quadrupole mass spectrometry52, 53 or
HTO radioactive tracers.54, 55
Although the Ca test has high sensitivity, there are numerous assumptions employed to
extract WVTR values from Ca test experiments. One assumption is the linearity of the optical
transmission, electrical conductance or oxidized area with Ca film oxidation. This assumption of
linearity has not been independently confirmed and must be questioned given recent evidence
for the inhomogenous oxidation of Ca films.56 Another assumption is the final oxidation state
of the Ca film. Both Ca(OH)2 and CaO are possible and could affect the WVTR value by a factor
of two.34, 57, 58
Another difficulty is the presence of residual H2O and H2O that enters the test apparatus
and oxidizes the Ca film without passing through the barrier. WVTR values as low as 5 x 10-5
g/m2/day at 38C/85%RH were measured for Al2O3 atomic layer deposition (ALD) films using
the Ca test with optical transmission probing.57 However, glass lid control experiments
indicated that these WVTRs were limited by H2O permeability through the epoxy seal.57
In this study, we employed several Ca test configurations to evaluate the gas diffusion
barrier properties of Al2O3 ALD films. Recent studies have shown that Al2O3 ALD films are
effective gas diffusion barriers and encapsulation layers.55, 57, 59-63 For this investigation, Al2O3
ALD films were deposited directly on Ca films using an ALD reactor that was accessed from an
N2-purged glove box. The Ca films were then probed by photographic imaging and electrical
conductance. Because the Al2O3 ALD films were directly deposited on the Ca film, the
photographic imaging can observe spatial information and locate defects in the Al2O3 ALD film.
![Page 47: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/47.jpg)
35
Electrical conductance measurements can also be performed concurrently with the
photographic imaging to correlate the spatially inhomogeneous Ca film oxidation with the
electrical behavior.
Experimental
Ca Deposition Using Glove box with Attached PVD Chamber
The Ca test requires that the Ca film be deposited and prepared for the gas diffusion
barrier measurements under a controlled oxygen-free environment. To meet this requirement,
an apparatus was built consisting of a physical vapor deposition (PVD) chamber connected to a
N2 glove box. The glove box was an Omni-Lab system from Vacuum Atmospheres Company
with a custom attachment ring welded into the floor of the unit. An ALD reactor was connected
to the bottom of the glove box using the attachment ring. Samples could transfer directly from
the N2 glove box to the ALD reactor using a Viton-sealed, quick-access door. This apparatus is
shown in Figure 1.10.
To prepare the Ca films, 3” x 1” glass slides were first placed in base piranha solution for
initial cleaning and then washed with water, acetone and methanol. While still in a methanol
bath, they were placed in a HEPA particle-filtered hood and then blown dry with N2. Double-
sided tape was used to attach stainless steel masks to the glass slides. The masks covered a
0.5” strip down the center line of the glass slide and left a 0.25” section on either side to be
coated with gold (Au) on a chromium (Cr) adhesion layer. The slides were then placed inside
the PVD chamber.
![Page 48: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/48.jpg)
36
The PVD chamber was pumped with a turbomolecular pump that maintained a typical
base pressure of 3 x 10-6 Torr. The PVD chamber contained a RF-Magnetron Torus source from
Kurt J. Lesker for sputter deposition. This source was powered by an Advanced Energy RFX-600
radio frequency supply with an ATX-600 matching network. Cr and Au were sputtered to
deposit ~110 nm of Cr and then ~130 nm of Au. After the Cr and Au deposition, the coated
slides were washed with acetone and methanol to remove the adhesive residue. The glass slide
was then cut into three 1”x1” squares.
The 1” x 1” squares were mounted onto a custom sample platter and masked for Ca
deposition in an area with dimensions of 0.75” x 0.5”. The platter was inserted into the PVD
chamber and the samples were attached to a rotating spindle. A pre-sputter of 1-2 minutes
was first performed with the substrate shielded to remove CaO from the Ca target. The
substrate was then uncovered and a Ca film was deposited using 300 W of forward power and
an Ar pressure of 15 mTorr. These conditions resulted in a Ca film deposition rate of
approximately 4.5 Å/s. The samples were then returned to the N2 glove box. The Ca films were
opaque with a mirror-like appearance. A top view schematic of these Au/Cr and Ca-coated
samples is shown in Figure 2.1.
The Ca film thickness was determined using focused ion beam (FIB) and scanning
electron microscopy (SEM) on reference samples using a NOVA 600i FIB/SEM from FEI. The
reference samples were prepared by depositing Ca metal on Si wafers. The Ca film was covered
with 110 nm of Cr to protect the Ca film from oxidation. Cross-sections of these samples were
![Page 49: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/49.jpg)
37
prepared using the FIB. Subsequently, cross-sectional SEM images measured a thickness of 270
nm for the Ca film.
To determine the purity of the deposited Ca films, the measurement samples were
analyzed by XPS depth-profiling. This analysis was performed using a PHI 5600 XPS instrument
with an Ar ion sputter gun. These XPS measurements determined that the Ca films contained
20 at.% O. CaO and Ca(OH)2 are insulating materials and will increase the Ca film resistivity.
The resistivity of the Ca films was determined by 4-wire resistance measurements
performed inside the glove box. A thicker Cr film thickness of ~540 nm without any Au
overlayer was used for these measurements. The resistance was then plotted as a function of
1/thickness. The Ca film thicknesses of 270, 410 and 570 nm were obtained by measurements
on reference samples using FIB/SEM analysis as described above. The slope of the plot of
resistance versus 1/thickness was then used to determine the film resistivity using R= l/A
where R is resistance, is resistivity, l is the length of the film and A is the cross-sectional area
of the film. A resistivity of ρ = 1.34 x 10-4 cm was obtained for these Ca films containing 20
at.% O. In addition, the y-intercept yielded a resistance of 0.23 that measures the resistance
in series to the Ca film.
![Page 50: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/50.jpg)
38
Figure 2.1 Top and side views of Ca film on Au/Cr metal electrodes on glass.
![Page 51: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/51.jpg)
39
Al2O3 ALD and ALD Reactor The Au/Cr and Ca-coated samples were then placed in the ALD reactor via a quick access
door on the floor of the glove box. The ALD reactor was a hot-wall, viscous flow ALD reactor
similar to reactors that have been described earlier.64
The reactants were alternately injected into
the ultrahigh purity N2 viscous flow carrier gas continuously traveling through the reactor. The
baseline chamber pressure was 650 mTorr with N2 flowing through the reactor. The reactant
pressures were both 300 mTorr.
Al2O3 ALD was performed using Al(CH3)3 and H2O as the reactants at 120 °C. The two
sequential, self-limiting reactions during Al2O3 ALD are:65, 66
(A) AlOH* + Al(CH3)3 → AlOAl(CH3)2* + CH4 (2.1)
(B) AlCH3* + H2O → AlOH* + CH4 (2.2)
where the asterisks indicate the surface species. This sequence defines one AB cycle for Al2O3
ALD. The timing for this sequence was (t1, t2, t3, t4) where t1 is the TMA exposure time, t2 is the
N2 purging time, t3 is the water exposure time and t4 is the second N2 purging time. The timing
sequence was (1.5, 75, 0.5, 75) where the time are in seconds. The repetition of these AB cycles
Humidity Chamber, Electrical Conductance, and Photographic Measurements After the desired barrier thickness was deposited, the Al2O3 ALD-coated Ca samples
were removed from the ALD reactor and N2 glove box. A side view schematic of these Al2O3
ALD-coated samples is shown in Figure 2.1. The samples were then placed into an oven at 70°C
containing a saturated MgCl2 solution that establishes the relative humidity of H2O within the
oven at ~28%. This method of setting relative humidity is widely used to calibrate humidity
![Page 52: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/52.jpg)
40
sensors.67, 68 The oven also had electrical feedthroughs and a viewport to view the Ca film
during the H2O exposure.
The electrical conductance of the sample was monitored with a Keithley 2400 digital
multi-meter connected to a computer. A custom Labview program was used to record the
sample conductance four times in every one second. The measurements were then averaged
to attenuate any electrical noise present in the signal. A USB camera was also positioned at the
oven viewport to monitor the sample visually. Image capture software (Flix by Nimisis) was
used to record a sample image every five minutes for the duration of the sample test. The
software was then used to process the photos into a time lapse video of the sample. This video
can monitor the evolution of sample oxidation.
Approximately 30 individual Al2O3 ALD-coated Ca films were evaluated during the
course of these experiments. Videos were recorded for 21 of these samples. All of the samples
displayed similar behavior for both the photographic images and electrical conductance. The
results described below will concentrate on one sample in detail. This sample is representative
of the entire set of samples.
Results
Photographic Images
Photographic images of the Ca film with a thickness of 270 nm coated with an Al2O3 ALD
barrier versus time at 70°C/28% RH are shown in Figure 2.2. This Al2O3 ALD film was grown
using 150 ALD cycles and had a thickness of 18.7 nm. The Ca film and the Au/Cr contacts on the
sides are clearly visible. The metallic Ca film appears dark in the photograph because of the
metallic Ca film reflectivity. The oxidized Ca film appears as a white area because the oxidized
![Page 53: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/53.jpg)
41
Ca film is transparent to light. The Au/Cr contacts on the sides of the Ca film are clearly
distinguished because they have a different reflectivity and color than the Ca film.
The photographic image of the Ca film in Figure 2.2A shows the presence of a few
circular spots in the Ca film after 23.6 hours. After 30.6 hours, Figure 2.2B shows that these
circular spots have grown and a few additional new small circular spots are noticeable. The
circular spots are identified as oxidized Ca regions. The video images clearly indicate that these
oxidized Ca regions are circular areas that grow radially in size versus time. This behavior
argues strongly for the existence of pinhole defects in the Al2O3 ALD coating on the Ca film.
These pinhole defects are believed to be caused by particles on the initial Ca film.69, 70
After 37.0 hours, the photographic image in Figure 2.2C shows that a large number of
new circular spots appear in the Ca film. This burst of new circular spots is also associated with
pinhole defects in the Al2O3 ALD barrier because the circular spots grow radially versus time. To
characterize this rapid “blooming” of circular spots, the number of circular spots appearing on
the entire sample was counted versus time. These results are shown in Figure 2.3. A large
increase in the number of circular spots was observed at ~32 hours at 70°C/28% RH. This
blooming may be due to water traveling through hydroxyl defects in the Al2O3 ALD film.
Experiments on films with smaller Al2O3 ALD thicknesses grown using 80 and 100 ALD cycles
observed the blooming at earlier times.
![Page 54: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/54.jpg)
42
50
40
30
20
10
0Nu
mb
er
of
Circu
lar
Sp
ots
3020100Time (hr)
70°C / 28 %RHAl2O3 Thickness = 18.7 nm
Figure 2.3 Number of circular spots on Ca film versus time for Al2O3 ALD film with thickness of 18.7 nm at 70 °C/28% RH. The rapid increase or “blooming” in number of circular spots occurs at ~32 hr.
Figure 2.2 Photographic images of Ca films with thickness of ~270 nm coated with Al2O3 ALD barrier with thickness of 18.7 nm at 70 °C/28% RH: (A) 23.6 hr; (B) 30.6 hr; (C)37.0 hr; and (D) 55.0 hr.
![Page 55: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/55.jpg)
43
The circular spots continue to grow and then grow together. After 55.0 hours, the
photographic image in Figure 2.2D shows the nearly complete oxidation of the Ca film. There is
also texture in the oxidized regions that is consistent with circular spots overlapping to form
larger oxidized areas in the Ca film. The texturing may also result from the progressive
expansion of the oxidized Ca film. The reaction of water with Ca metal to form calcium
hydroxide (Ca(OH)2) results in a 27% increase in volume. Calcium hydroxide can also readily
react with CO2 to form calcium carbonate (CaCO3). This reaction results in a further increase in
volume to a total of 31% (aragonite) or 42% (calcite) above the original Ca volume.
Electrical Conductance
Electrical conductance data was collected concurrently with the photographic images.
Figure 2.4 shows the conductance for the same Ca film that was analyzed using photographic
images in Figure 2.2. The electrical conductance at (A) 23.6 hours, (B) 30.6 hours, (C) 37.0 hours
and (D) 55.0 hours correspond with the photographic images in Figure 2.2. The loss in
conductance is not linear in time. The conductance initially shows almost no change versus
time on this sample and the other samples. At 23.6 hours labeled as (A), the conductance is on
the threshold of a large reduction. Figure 2.4 shows that the large conductance drop occurs at
~30 hours. This conductance drop coincides closely with the sudden increase in the number of
circular spots on the Ca film that appears as a “blooming”.
![Page 56: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/56.jpg)
44
0.10
0.08
0.06
0.04
0.02
0.00
Conducta
nce (
mho)
6050403020100Time (hr)
A
BC
D
090325
Figure 2.4 Conductance versus time for Ca film with thickness of ~270 nm coated with Al2O3 ALD barrier with thickness of 18.7 nm at 70 °C/28% RH. The locations A, B, C and D
correspond with photographic images in Figure 2.2.
![Page 57: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/57.jpg)
45
At 30.6 hours labeled as (B) in Figure 2.4, the number of circular spots is starting to
increase suddenly in Figure 2.3 and the conductance has reduced to approximately half of its
initial value. Figure 2.4 shows that the conductance drops to less than 10% of its initial value in
very close correspondence to the end of the sudden “bloom” in Figure 2.3. At times after the
“bloom”, the electrical conductance is approximately constant. Concurrently, the photographic
images show that the circular spots are beginning to intersect with each other as displayed in
Figure 2.2C. At later times, the circular spots continue to grow and cover most of the Ca film.
In this regime, as illustrated photographically at 55.0 hours in Figure 2.2D and labeled as (D) in
Figure 2.4, the conductance is zero because there are no conducting pathways in the Ca film.
The electrical conductance in Figure 2.4 is assumed to be dominated by the Ca film with
no series resistance.56 This assumption is reasonable because the resistivity measurements of
Ca films using thicker Cr film thicknesses of ~540 nm yielded a series resistance of only 0.23 .
For the Cr adhesion layer film thickness of ~110 nm with the Au overlayer film thickness of ~130
nm, the series resistance is expected to be even smaller than 0.23 This series resistance is
negligible compared with the measured resistance of ~10 for the initial Ca film samples.
WVTR from Electrical Conductance
Under a certain set of assumptions, WVTR values can be determined from the time-
dependence of the electrical conductance. Assuming that the electrical conductance is linear
with Ca film oxidation, the conductance method can derive the WVTR from the change of
conductance versus time.34 Under this assumption and assuming that the Ca film oxidizes to
Ca(OH)2 purely by reaction with water, this method was used to determine WVTR values from
the conductance curve in Figure 2.4.
![Page 58: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/58.jpg)
46
The WVTR or permeation rate, P, is determined using:34
( )
( )
( )⁄
(2.3)
In Eq. 2.3, n is a stoichiometric coefficient which is n=2 for water oxidation, M(Ca)= 40.078
g/mol is the molar mass of Ca, and M(reagent)= 18.015 g/mol is the molar mass of H2O. = 1.54
g/cm3 is the bulk density of Ca and ρ = 1.34 x 10-4 cm is the resistivity of Ca film. b=1.27 cm
is the width of Ca film and l =1.27 cm is the separation of between the Au/Cr contacts. In
addition, 1/R is the measured conductance (mho).
The resulting WVTR values are given in Figure 2.5. The WVTR values are fairly constant
at WVTR ~2 x 10-2 g/m2/day in the initial portion of the conductance curve at times <30 hours.
These WVTR values are higher than previous WVTR values of ~1 x 10-3 g/m2/day for Al2O3 ALD
films on PEN polymer substrates measured at 25°C/100 %RH using the HTO isotope method.55
These WVTR values are also much higher than the WVTR values of 1.7 x10-5 g/m2/day and 6.5
x10-5 g/m2/day at 38°C/85 %RH and 60°C/85 %RH, respectively, for Al2O3 ALD on PEN polymer
substrates measured using the optical Ca test.59 The differences between the HTO and Ca test
methods were attributed to T/H exchange on hydroxyl groups and T diffusion through the Al2O3
ALD barrier.71 The T diffusion limits the lowest WVTR value that can be measured using the
HTO method.71
![Page 59: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/59.jpg)
47
0.10
0.08
0.06
0.04
0.02
0.00
Co
nd
ucta
nce (
mh
o)
6040200Time (hr)
10-8
10
-6
10
-4
10
-2
10
0
WV
TR
(g
/m2/d
ay)
090325
Figure 2.5 WVTR values corresponding with conductance versus time for Ca film with thickness of ~270 nm coated with Al2O3 ALD barrier with thickness of 18.7 nm at 70 °C/28% RH.
![Page 60: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/60.jpg)
48
The higher WVTR values for Al2O3 ALD films deposited directly on Ca films may result
from chemical interactions between the Al2O3 ALD film and the Ca film that may degrade the
Al2O3 ALD film. Calcium in the form of calcium oxide (CaO) or calcium carbonate (CaCO3) is
known to react with Al2O3 at high temperatures to form calcium aluminate (CaAl2O4).72, 73 The
higher WVTR values may also result from the rough surface morphology of the sputtered Ca
film or particles on the Ca film that lead to more defects in the Al2O3 ALD film.
The WVTR values in Figure 2.5 obtained from the electrical conductance measurements
increase when the conductance falls at ~30 hours. The largest WVTR values are observed at the
time of the “bloom” when the number of circular spots increases dramatically at 32-35 hours.
As the oxidation areas on the Ca film begin to merge, the electrical conductance falls to nearly
zero and the conductance measurements can no longer yield an accurate WVTR value. In this
regime, there are few electrical conduction pathways that transverse the Ca film. The relative
change of the conductance is small and the WVTR values derived from Eq. 3 are extremely low.
WVTR from Photographic Images
The WVTR values were also obtained from the photographic observations. This
determination was accomplished using ImageJ software to convert color images from the USB
camera to black-and-white images. The color images were first converted to grey-scale images.
A grey-scale threshold value was then set to produce binary images of black-and-white pixels.
The grey-scale threshold value was determined visually based on a comparison between the
color image and the black-and-white image. Examples of these high contrast black-and-white
images are shown in Figure 2.6.
![Page 61: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/61.jpg)
49
Figure 2.6 High contrast black-and-white images of Ca film with thickness of ~270 nm coated with Al2O3 ALD barrier with thickness of 18.7 nm at 70 °C/28% RH.
![Page 62: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/62.jpg)
50
Based on this procedure, ImageJ was then able to provide an accurate measurement of
the white areas that correspond to oxidized Ca film. Similar approaches have been employed
to measure the amount of oxidized Ca using optical microscopy.16 In some instances, poor
resolution and sample lighting led to inaccuracies in the converted photographic images. For
example, very shiny metal areas could appear as white oxidized areas. These errors could be
minimized through careful observation and manually removing the reflections from the
measured oxidized area.
The white oxidized surface areas could be converted to the amount of Ca film oxidation.
The conversion between the white area and Ca film oxidization assumed that the Ca film was
oxidized laterally as shown in Figure 1.8. The white circular areas grow radially versus time as
the Ca film is oxidized by H2O traveling through a pinhole defect. The Ca film was assumed to
be completely oxidized in the white areas. This assumption is reasonable because the Ca film
has a thickness of only ~270 nm that is much smaller than the typical size and change of
diameter of the circular spots.
The WVTR, or permeation rate, P, is determined from the photographic images using:
( )
( )
(2.4)
In Eq. 2.4, n, M(H2O),M(Ca) and are the same as in Eq. 2.3. The change in oxide area is
represented by ΔA. The time interval, in days, between the photos used to measure ΔA is
represented by Δt. h= 270 nm is the height of Ca metal film. The WVTR values obtained from
![Page 63: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/63.jpg)
51
the photographic image analysis of the Ca films is shown in Figure 2.7. The WVTR values
obtained from the electrical conductance results are also shown for comparison.
The WVTR values obtained from the electrical conductance measurements are
somewhat higher than the WVTR values derived from the photographic image analysis.
However, considering all the assumptions in the determination of the WVTR values and the
inhomogeneous change of the Ca film during oxidation,56 this agreement within an order of
magnitude is promising. In particular, the relationship between the oxidized area of the Ca film
and the decreasing electrical conductance may be very complex.
The WVTR values derived from the photographic images and the electrical conductance
are not in good agreement at later times after the “blooming” at 30-32 hours. This lack of
agreement is not surprising. The circular spots are beginning to grow together on the Ca film
and the electrical pathways across the Ca film are being severely restricted. The conductance
values are approaching zero at >32 hours and the small time derivatives lead to artificially low
WVTR values from the electrical conductance.
![Page 64: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/64.jpg)
52
10-5
10-4
10-3
10-2
10-1
100
WV
TR
(g
/m2/d
ay)
40353025201510
Time (hr)
090325
Electrical Conductance
Photographic Image
Figure 2.7 Comparison between WVTR values obtained from photographic image and electrical conductance analysis versus time.
![Page 65: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/65.jpg)
53
Discussion
WVTR Measurements Using the Ca Test Because there are no commercial instruments that can measure ultralow WVTRs, most
efforts have relied on the oxidation of metallic Ca films to determine H2O permeability rates.
Because the oxidation of metallic Ca leads to a transparent and insulating film, the methods of
employing the Ca test have been to measure the optical transmittance of the Ca film, the
electrical conductance of the Ca film, or the oxidation area of the Ca film versus time. The
optical transmittance method was described by Nisato et al. in 2001.51 The electrical
conductance method was demonstrated by Paetzold et al. in 2003.34 The oxidized area method
was introduced by Kumar et al. in 2002.16
Various groups have used the Ca test with the optical transmission method to measure
the WVTR.51, 57-59, 74 Other groups have employed the Ca test with the electrical conductance
method to measure the WVTR.34, 56, 75, 76 Additional studies have used the oxidation area of the
Ca film to derive the WVTR.12, 16, 51, 77, 78 A wide range of WVTR values is obtained from all of
these measurements. Attempts to understand the reliability of the WVTR values is not easy
because most of the Ca test studies have not been described in detail. In addition, many of the
assumptions of the optical transmission, electrical conductance or oxidation area methods have
not been clearly defined or verified by these studies.
Our combined studies using the photographic image and the electrical conductance of
the same Ca film help to check the validity of the WVTR measurements. Figure 2.5 shows that
the WVTR values determined using the electrical conductance vary considerably depending on
the oxidation of the Ca film. Initial WVTR values of ~2 x 10-2 g/(m2*day) at times between 10-20
![Page 66: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/66.jpg)
54
hours are somewhat larger than previously measured WVTRs for Al2O3 ALD films.55, 59 However,
after the “blooming” of the Ca film, the WVTR values change dramatically. They first increase
several orders of magnitude and then plummet as the electrical conductance approaches zero.
The comparison between the WVTR values obtained by the photographic images and
the electrical conductance can be used to determine the regions were the WVTR values are in
agreement. Figure 2.7 shows that the WVTR values obtained prior to the “blooming” of the Ca
film are in reasonable correspondence. From 10-30 hours, the WVTR values are similar to
within an order of magnitude. The electrical conductance WVTR values are consistently higher.
Another check on the reliability of the WVTR value can be obtained by using the total
time for the electrical conductance to reach zero. Knowing the thickness of the Ca film and the
initial composition of the Ca film, the oxidation of this Ca film to Ca(OH)2 can be converted to a
WVTR value. Based on the ~33 hours required for the electrical conductance in Figure 2.4 to be
reduced to <10% of its initial value for a Ca film thickness of ~270 nm, the WVTR value is ~0.2
g/(m2*day). This determination considered that the Ca film was 20 at.% O. This WVTR value is
comparable with the largest WVTR values obtained by the electrical conductance or
photographic image analysis after the onset of the “bloom”.
The wide range of WVTR values obtained by these different methods for the same set of
data raises serious questions about the reliability of the Ca test methods. The lack of
consistency suggests that the Ca film oxidation may not be simple. The electrical conductance
may not be linear with oxidation as usually assumed by previous studies. The Ca film oxidation
may not occur as assumed by the mechanism presented in Figure 1.8. We note that other
![Page 67: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/67.jpg)
55
recent studies of the morphology of the Ca films upon H2O exposure have revealed that the
oxidation is not homogenous.56 The Ca film may not oxidize linearly from top to bottom. The
inhomogeneous nature of Ca film oxidation may affect the dependence of the electrical
conductance and the oxidized area on Ca film oxidation.
Nature of Pinhole Defects Observed By Ca Test
The deposition of the Al2O3 ALD films directly on the Ca film allowed the defects in the
Al2O3 ALD film to be directly visualized. This method is similar to previous studies that have
deposited gas diffusion barriers directly on polymer films and then used an O2 plasma to
visualize the defects. The atomic oxygen in the O2 plasma etches the polymer through the
defect and the undercutting can be observed using optical and electron microscopy.70, 79
Depositing the Al2O3 ALD film directly on the Ca film also is similar to experiments where the Ca
film is deposited on a polymer substrate and the barrier is deposited on the other side.12, 16, 77, 78
In this case, the Ca degradation can identify the location of the defect in the barrier on the
other side of the polymer. Other studies have also recently been developed to view individual
defects in Al2O3 ALD films using copper electroplating or fluorescent tagging.80, 81
These current studies revealed that there are two types of pinhole defects that
appeared and grew circularly versus time. The first type of pinhole defects are the defects that
are present initially in the photographic images. Examples of these pinhole defects are shown
in Figure 2.2A. We believe that these defects are associated with particles on the initial Ca
film.69, 70 The particles are believed to mask the underlying Ca film from Al2O3 ALD and lead to a
pinhole defect in the Al2O3 ALD film.
![Page 68: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/68.jpg)
56
The second type of defects is associated with the “blooming” of oxidation areas that are
observed at later times. These defects appear very suddenly versus time. An example of the
“blooming” of oxidation areas is shown in Figure 2.2C. These defects have the characteristics of
pinhole defects because they grow circularly versus time. However, these defects develop in
the Al2O3 ALD film at later time and the onset time depends on the Al2O3 ALD film thickness.
We believe that these defects are caused by water corrosion of the Al2O3 ALD film. Another
possibility is that these defects result from the chemical interaction between the Al2O3 ALD film
and the Ca film.
The nature of the defects caused by water corrosion may be similar to the defects
described in recent studies of H2O permeation in Al2O3 ALD films of different thicknesses grown
at different temperatures.82 This study postulated that H2O transport through Al2O3 ALD films
occurs by H2O permeating along percolation paths formed by OH-defect clusters.82 A certain
fraction of these HO-defect clusters exist in Al2O3 ALD films. Permeation will occur when a
percolation path exists across the full thickness of the Al2O3 ALD film.83, 84 The probability that
such a percolation path will exist increases as the Al2O3 ALD film thickness decreases.
For the current studies, the “blooming” occurs at a time when there are percolation
paths across the Al2O3 ALD film resulting from H2O corrosion. These percolation paths are not
believed to exist initially at early time. These percolation paths are formed progressively with
time resulting from H2O corrosion of the Al2O3 ALD film. Previous studies have revealed that
nanoporous aluminum oxide films are susceptible to moisture induced degradation.85, 86 Other
studies have observed that Al2O3 ALD films are susceptible to H2O corrosion.71, 87 Al2O3 ALD
![Page 69: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/69.jpg)
57
films are also known to dissolve in liquid H2O.88 The “blooming” observed in these studies may
be another indication of H2O corrosion.
Conclusions Ca films were employed to evaluate gas diffusion barriers grown using Al2O3 atomic
layer deposition (ALD). The Al2O3 ALD barriers were grown directly on Ca films. The oxidation
of the Ca films was then monitored by measuring the electrical conductance of the Ca film or by
recording the photographic image of the Ca film. The photographic images revealed that the
Al2O3 ALD films have a small number of pinhole defects. These pinhole defects produce Ca film
oxidation areas that grow radially around the pinhole defect versus time. These pinhole defects
are probably caused by particles on the initial Ca film. The photographic images also observed
a burst of new circular oxidation areas that appeared suddenly at later times and grew radially
versus time. These defects may be caused by water corrosion of the Al2O3 ALD films.
The electrical conductance of the Ca film initially displayed little change versus time.
The correlation between the photographic images and the electrical conductance showed that
the conductance dropped when the circular oxidation areas in the photographic images
became a noticeable fraction of the Ca film area. The conductance measurements yielded a
WVTR value of ~2x 10-2 g/m2/day before the reduction of the conductance. The WVTR values
obtained from the electrical conductance and the photographic images were in approximate
agreement and increased versus Ca film oxidation until the rapid “blooming” of new circular
oxidation areas. WVTR values were also estimated from the time required for the electrical
conductance to be reduced to <10% of its initial value. These estimated WVTR values of ~0.2
g/m2/day were similar to the largest WVTR values obtained from the electrical conductance and
![Page 70: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/70.jpg)
58
the photographic images after the onset of the “blooming”. These results reveal the range of
WVTR values that can be obtained from different variations of the Ca test and the dependence
of the WVTR values on Ca film oxidation.
![Page 71: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/71.jpg)
59
Chapter 3 A New Calcium Test Apparatus
Abstract Ultralow permeability gas diffusion barriers on polymers with water vapor transmission
rates (WVTRs) as low as <10-6 g/(m2*day) are required for organic electronic and thin film
photovoltaic devices. The Ca test is the only technique with sufficient sensitivity to measure
these ultralow WVTRs. WVTR values as low as 5 x 10-5 g/(m2*day) have been measured for
Al2O3 atomic layer deposition (ALD) films at 38C/85% RH using the Ca test with optical
transmission probing.13 However, glass lid control experiments indicated that these WVTRs
were limited by H2O permeability through the epoxy seal. Several new implementations of the
Ca test were explored to overcome the limitations caused by epoxy seals. However, the
electrical conductance changed dramatically when the oxidized areas of Ca prevented electron
conduction across the Ca film. The design described here measured the electrical conductance
of Ca films in a test chamber that does not require epoxy seals. In this case, the polymer films
were attached to the test apparatus using differential seals. All components in the apparatus
were also baked in vacuum to remove any residual H2O. This new test setup has yielded a
baseline WVTR of 2.5 x10-4 g/(m2*day) which is a slight improvement on current commercial
instruments. The new instrument has the added potential of measuring OTR and WVTRs
independently.
Introduction The calcium test uses a thin, metallic, calcium layer as a sensor for water and oxygen
permeation.9, 12, 13, 16 There are two versions of the Calcium test, both of which rely on
measuring the oxidation of Ca metal. 33, 34 The main difference in the methods is how the Ca
![Page 72: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/72.jpg)
60
oxidation is measured. As oxygen or water permeate the barrier, they react with Ca to form
calcium oxide [CaO] or calcium hydroxide [Ca(OH)2], both of which are transparent to visible
light and electrically insulating.
In 2001, Nisato et. al described a testing method using calcium (Ca) metal for measuring
low H2O and O2 permeation rates.33 Their tests relied on using optical observations of the
oxidation of metallic Ca to Ca(OH)2 and CaO to determine calcium corrosion rates. A CCD
camera was used to monitor the reflection from Ca pad. From the images obtained they
measured the area growth of local oxidation regions. Once the growth rate of these areas
becomes linear they use that rate to determine WVTR. These measurements allow the
calculation of the overall degradation rate of the calcium layer and the permeation rate for the
barrier. The WVTR and OTR cannot be easily separated by this method. Further small error is
introduced by the difference in optical constants between the CaO and Ca(OH)2 products.
However, this method is useful to get a baseline measurement of the barrier performance. .
The % transmittance of the sample can also be followed as a function of time. However, the
development of localized oxidation regions will result in sudden increases in the transmittance.
The non-uniformity of the Ca degradation can lead to errors in the determination of a WVTR.
Other groups have subsequently employed the Ca test with optical transmission
probing to measure gas diffusion barriers.35 A similar Ca test method was recently used by
DuPont to evaluate Al2O3 ALD barriers on polymer substrates.13 An illustration of the Ca test at
DuPont is shown in Figure 1.5.13 The barrier film is adhered to the Ca test films on a glass
substrate using an epoxy seal. The Ca test revealed that the Al2O3 ALD film was an excellent
![Page 73: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/73.jpg)
61
barrier and WVTR values less than 5 x10-5 g/(m2*day) were obtained at 38 °C/85% relative
humidity (RH).36
A second implementation of the Ca test has also been developed that relies on
measuring the electrical conductance of a Ca film during oxidation.34, 37 In this version of the Ca
test, samples can be prepared by depositing Ca metal on a polymer substrate or directly on the
barrier. A schematic of the experimental configuration adapted from Ref. 34 is shown in Figure
1.6. Silver contacts were evaporated and the sample was covered with a glass lid using an
epoxy seal.
Problems with the Ca Test
There are some limitations of the optical implementation of the Ca test. In particular,
the Ca test is limited by the epoxy edge seal that provides a path for H2O and O2 diffusion.
Recent tests have revealed that Al2O3 ALD barriers on PEN were equivalent to the glass lid
control with using optical Ca test.36 The measured water vapor transmission rate (WVTR) for
both the Al2O3 ALD film and the glass lid yielded effective WVTR values of ~1x10-4 g/(m2*day).
This WVTR value was assigned to H2O permeation through the epoxy edge seal.36 With such a
high baseline WVTR value, the Ca test cannot easily be used evaluate high quality, low
permeability barriers with a WVTR values at or below 5x10-5 g/(m2*day) at 38 °C/85% RH. The
largest limiting factor for the electrical Ca test is also the epoxy edge seal.
There are other problems with the Ca test using either the optical and conductance
methods. In addition to the epoxy edge sealing, another issue that affects the optical method is
the required modeling of the optical multilayer stack. The modeling is difficult because of a lack
![Page 74: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/74.jpg)
62
of knowledge regarding the identity of the oxidized Ca sample. The oxidized Ca could be either
CaO or Ca(OH)2 and their optical constants are not known exactly. An unknown, changing,
mixture of the two, which will vary through the test, further complicates the modeling. This
variance is caused by the reaction sequence that Ca metal undergoes when exposed to water
and oxygen. If Ca metal is exposed to oxygen first, it will form CaO (ΔHfo=-635.09 kJ/mol). If the
CaO is sequentially exposed to H2O will with form Ca(OH)2 (ΔHfo=-986.09). Since only the first
change from metal to oxide (or hydroxide) causes a conductance change this means the two
permeation rates cannot be separated. The typical solution to this is that all oxidation is
assumed to be due to water permeation and an “effective WVTR” is typically reported. The
optical method suffers further from multiple optical layers with varying properties that are not
known accurately. These layers include the glass substrate, the epoxy, and the polymer. In
addition, the gluing of the polymer to the Ca film on the glass substrate using epoxy means that
the polymer cannot be reused after the Ca test. Consequently, many individual samples are
required to obtain meaningful results.
Other difficulties affect the Ca test using the conductance method. The conductance
test assumes that uniform Ca oxidation occurs in a top-to-bottom fashion. 34 Since barrier
permeation is known to be defect-dominated, uniform Ca oxidation may not be occurring if the
Ca film is located close to the barrier.14, 38, 39 This is the original configuration that has been
widely used. In the case of pinhole defects, the Ca film may be oxidizing in localized areas
under the pinhole defects. Depending on the distribution of defects, large conduction paths
can become electrically isolated without oxidizing all of the Ca metal in the electrical path. Such
situations result in a sharp decrease in conductance resulting from the restricted percolation
![Page 75: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/75.jpg)
63
path rather than true Ca oxidation. Oxidation via pinholes occurs in a hemispherical fashion. As
long as the radius of the hemisphere is smaller than the thickness of the Ca film the electrical
method provides a meaningful result.
A second problem for the conductance method arises from the metal used to form the
electrical contacts with the Ca metal. Silver and gold are common choices for good electrical
contacts that will not corrode. Unfortunately, both of these metals form crystalline alloys with
Ca at temperatures where the permeation tests are conducted.40, 41 There are multiple alloy
phases that can form, all of which have exothermic enthalpies of formation ranging from -41 to
-106 KJ/mol.42 These alloys are typically studied at elevated temperatures. However, recent
results have shown that annealing at relatively low temperature (270 °C) for as little as 15
minutes can affect Au-Ca alloy structure.43 This alloy formation leads to changes in the
conductance measurement that cannot be accounted for and increases the uncertainty in the
measurements. Other metals besides silver and gold must be employed to avoid this difficulty.
After noticing this problem with gold contacts we determined that Cr metal made an
appropriate electrical contact.
Ca Test Electrical Model
We will be using the equation originally published by Paetzold in 2003 with some of our
own modifications. The original equation is:
( )
( )
( )⁄
P = Permeation Rate (g/(m2*day)); n = stoichiometric coefficient; M(Ca) = Molar mass of Ca; M(reagent) = Molar mass of H2O or
O2; δ = density of Ca; ρ = resistivity of Ca; l = separation of contacts; b = width of Ca pad; 1/R = Conductance (mho)
![Page 76: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/76.jpg)
64
This model makes a few critical assumptions. First, that Ca corrosion is uniform in one
dimension, perpendicular to the barrier. Secondly, that all corrosion is due to either water or
oxygen. Third, the film is uniform in density and resistivity. The fourth and final assumption is
that the area of the Ca pad and the area of the barrier are equal. If the Ca sensor has significant
separation from the barrier, such as in our apparatus, the Ca and barrier areas must be
included. The modified equation would then become:
(3) ( )
( )
( )⁄
If we examine the assumptions we find a few problems. At first it seems reasonable
that, if the barrier is pinhole free, oxidants permeating the barrier will uniformly diffuse.
Barrier permeation is known to be defect-dominated.14, 33 If the barrier is oriented toward the
humid atmosphere the following happens. The oxidant permeates a pinhole and enters the
polymer; the concentration of water expands in all directions equally. This forms a
hemispherical wave that diffuses through the polymer (Figure 1.7). If the separation between
the defects is less than the polymer thickness the hemispheres will join. Once the hemispheres
join, a uniform wave front of water is formed. When this wave front reaches the Ca we would
expect it to also oxidize uniformly. For this to happen all of the defects must have a separation
less than the thickness. The model doesn’t hold true barrier defects act as point sources. If the
defects have very large separations the hemispheres will reach the Ca at individual points. The
Ca will begin to oxidize at that point. This process is even more pronounced when the Ca film is
directly on the barrier (Figure 1.8). The oxidation will spread in a hemispherical wave front
![Page 77: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/77.jpg)
65
through the Ca just at is did through the polymer. Once the hemisphere has moved to through
the calcium thickness the oxidation will expand in as a cylinder centered on the defect. As
oxidation progresses the edges of the cylinders will meet. Depending on the distribution of
defects, large conduction paths can become electrically isolated without oxidizing all of the Ca
metal in the electrical path. Such situations result in a sharp decrease in conductance resulting
from the restricted percolation path rather than true Ca oxidation. This makes difficult to
accurately determine a WVTR using the standard interpretation of Ca test conductance curves.
If the barrier is facing the atmosphere this could take days depending on the defect size
and separation. With the barriers facing the Ca sensor, polymer saturation should happen
within a day or two depending on experimental conditions and polymer substrate. Water
absorption by the polymer may lead to barrier disruption if the polymer expands.
The assumption of water being the major oxidant is made because limited results have
shown that the oxidation of the Ca varies greatly with temperature and humidity content. This
has led many to believe that water is the predominant penetrant. This may simply be that the
activation energy need for oxygen to react with a Ca surface is higher than H2O. No apparatus
has yet been built that can separate OTR and WVTR for barrier films. We did not perform these
experiments, but our apparatus could be easily adapted to. For the purposes of our work we
will be report the apparent WVTR for barrier films.
Experimental After the lessons learned from depositing Al2O3 ALD barriers on Ca we decided to use a
different tactic. We have developed a conductance Ca test apparatus that does not use an
![Page 78: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/78.jpg)
66
epoxy adhesive to seal the polymer substrate to the Ca test pad. Instead of an epoxy, a
differential seal is used to attach the polymer substrate and isolate the internal volume of the
Ca test apparatus from the outside. The main idea was to separate the Ca pad from the barrier
sample and to handle the barrier edge sealing separately from the Ca sensor attachment. The
apparatus went through much iteration in order to obtain a final design that would reach the
necessary baseline WVTR. Only the final design will be described here. The apparatus consists
of six pieces, most of which are custom made. These pieces are:
1. Base Plate and Sensor Holder 2. Electrical Ring (E-Ring) 3. Adapter Plate 4. Sample Cover 5. Shroud 6. Ca Sensor
Base Plate and Sensor Holder
The base plate is made from a standard 4-1/2” CF viewport. It is fitted with a custom
designed holder for the Ca sensor. The combination of viewport and sensor holder maintains
the sensors electrical contact and allows it to be visually monitored if desired with a USB
microscope. The first material chosen for the interior sensor holder was originally polyether
ether ketone (PEEK). PEEK was chosen because it is electrically insulating, easily machined and
can sustain high temperatures. While the material is a polymer and capable of absorbing water
we believed that the surface-gas equilibrium would be must faster than water absorption into
the bulk. With the Ca metal acting as a getter pump for the interior volume this seemed likely.
To reach a steady state measurement the interior surfaces must be in equilibrium with the
interior volume. However, when we began testing bare PEN samples we believed the lag times
![Page 79: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/79.jpg)
67
Figure 3.1 Base Plate with Sensor Holder (Top View)
![Page 80: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/80.jpg)
68
to be abnormally long. We tested whether or not the lag time would change if the sensor
holders were reused with or without baking between each test. We found that the lag time did
markedly decrease if the sensor holders were not baked and was reversible upon baking. As a
result we had the sensor holder remanufactured the out of stainless steel to remove this water
reservoir. This required some slight modifications to the design as well as the addition of
contact insulators. The contact insulators were made from Macor®, a non-porous machinable
ceramic that does not absorb water. The insulators allowed the fixing of the contacts against
the sensor without shorting to the apparatus body. This change added complexity but it
significantly reduced the lag time for the apparatus. Bases are baked for at least 24 hours at
120 °C under 1 torr of Ar or N2 prior to each use to ensure consistent results.
Electrical Ring
The electrical ring is made from a double sided 4-1/2” CF flange that has been modified
with copper electrical feedthroughs. Special copper contacts are permanently connected to the
interior of the feedthroughs. The contacts had to be shaped so that firm contact could be made
without the risk of breaking sensors during assembly. The sensitivity of the instrument to small
fluctuations in resistance requires some special steps in assembly. If these steps are ignored
the measurement will have significant noise. Thermocouple joints must be absolutely avoided
therefore solder connections cannot be used. The copper contacts are manufactured with a
press fit pin to attach a copper mesh. The mesh gives the contacts some flexibility to ease
assembly of the apparatus. The mesh is attached to a feedthrough using custom crimp
connectors. The same connectors are used on the exterior to connect the feedthroughs and
shield twisted pair wire. The shield is connected to the grounded faraday cage surrounding the
![Page 81: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/81.jpg)
69
Figure 3.2 Electrical Ring (Top View)
![Page 82: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/82.jpg)
70
Keithley instrument during an experiment. Exposure of the exterior feedthrough wire to the
salt water environment during initial testing caused stray voltages to appear. Most likely this
was due to the “tinned” twisted pair. Salt water forming a multilayer on the surface most likely
created a galvanic cell. Stray voltages were also seen, to a lesser extent, in the ESPEC
environmental chamber. Hermetic sealing is required to prevent a galvanic cell condition. The
twisted pair wire also needs support to prevent a short developing by repeated flexion during
handling. Initially, sealing and support were provided using Epoxy Technology 353ND epoxy
with a fiberglass skeleton. This was found to be functional but somewhat fragile. Our final
apparatus uses two HDPE “wings” that provide support for the wire leads and a form for the
epoxy encasement. The leads terminate in gold plated dual banana plugs that can be plugged
into the Keithley meter.
Adapter Plate
The adapter plate is designed with two concentric seal regions and bolt patterns for the
sample cover, shroud and electrical ring. The depth of the seal faces are carefully machined to
prevent over tightening of the sample cover but give a good seal. If the sample cover is over
tightened the barrier sample will be deformed and most likely damaged. Assembly will be
discussed later. The inner O-ring seal holds the barrier sample while the outer seal forms a
differential pumping region. The inner seals are designed to minimize mechanical strain on the
barrier sample by sandwiching it between two identical seals. Depending on the
barrier/substrate system even a relatively small mechanical strain could result in failure. By
avoiding strain the apparatus can test fragile barriers. The seals can separate from the sample
without causing damage; samples can then be retested to minimize experimental error.
![Page 83: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/83.jpg)
71
Figure 3.3 Adapter Plate (Top View)
![Page 84: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/84.jpg)
72
Dismantling outside of the glove box is necessary to reuse samples. Insertion into the glove box
means pump-purge cycles; this will flex and most likely break any barrier. Exposure to the
atmosphere of the interior volume would require a bake out before the apparatus can be
reused. With only a few test setups available we did not use this ability of the apparatus. The
outer O-ring seal is twice the thickness of a single inner seal which balances the force when the
sample cover is applied. The seals must be baked for at least 72 hours before they can be used
to remove absorbed water. Two ports mounted 180 degrees provide access to the pumping
region between the seals. Pumping and metered N2 lines are attached to these ports. The zone
is purged with a constant filtered flow of N2 from a liquid nitrogen tank for the duration of the
test. The N2 pressure within the interstitial zone is kept between 1-2 torr.
Sample Cover
The sample cover is the mirror image of the adapter plate with a center bore to allow
atmosphere access to the sample. A second sample cover, without a bore, is used as a control
lid to determine the leak rate through the edge seal. When the cover is bolted on the bolts are
tightened in an “every third bolt” pattern. They are first tightened to a low torque to align and
balance the seals. Next they are incrementally tightened to 8 in-lbs of torque to uniformly hold
the sample.
Shroud
The shroud seals around the sample cover and to the top adapter plate face with a
space for N2 to flow. It has inlet and outlet ports mounted 180 degrees apart. A metered N2
line is attached to the inlet via a shutoff valve; the second is left open to the humidity chamber
as an outlet. The interior of the shroud is flushed with a high flow of dry N2 above atmospheric
![Page 85: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/85.jpg)
73
Figure 3.5 Shroud (Bottom View)
Figure 3.4 Sample Cover (Bottom View)
![Page 86: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/86.jpg)
74
pressure for the duration of the test. This limits the partial pressure of the H2O/O2 challenge to
the edge of the seals.
Ca Sensor
The Ca sensor is made by starting with a 3” x 1” glass slide. The slides are base bathed
to remove any oils. After removal from the bath they are washed with water, acetone and
methanol. They are left in a methanol bath and placed under a HEPA particle hood. Once
under the hood they are blown dry with filtered N2. Double sided tape is used to attach
stainless steel masks to the glass slides. The masks cover a 0.5” strip down the center of the
glass slide, leaving a 0.25” section on either side to be coated with Chromium (Cr) metal.
Double sided tape is then used to attach multiple masked slides to a sample platter. The slides
are placed inside the PVD chamber and pumped down. Chromium metal is deposited using 400
watts with 15 mtorr partial pressure of Ar for 20 minutes (Table 1.1). This gives a contact
thickness of approximately 540 nm. Once deposition is complete the slides are removed and
unmasked. They are visually inspected for contact uniformity; any slides with defects are
discarded. The coated slides are washed with acetone and methanol to remove adhesive
residue. After being blown dry they are cut into three 1”x 1” squares. The newly made sensor
substrates are put into the glove box for the next steps. Immediately prior to each test run a
sensor substrate is placed onto a custom PVD sample platter and masked. The mask leaves a
0.75” by 0.5” area for Ca deposition. Care must be taken to ensure that the correct substrate
side is exposed. The platter is inserted into the PVD chamber via the transfer arm and gate
valve. Calcium pads were deposited using the conditions listed in Table 1.1; Ca deposition time
was typically 10 minutes. The sensors were then returned into the N2 glove box. From there
![Page 87: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/87.jpg)
75
Figure 3.6 Diagram of Ca sensor
![Page 88: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/88.jpg)
76
the sensors were assembled into the Calcium test apparatus. Calcium sensor substrates can be
re-used after being rinsed in a dilute H2SO4 solution and cleaned using the initial procedure.
This reduces the cost of maintaining the apparatus. Before reuse the contacts should be
inspected for scratches. Good even contacts are very important for preventing noise in the
conductivity.
Assembly Once the Ca sensor has been deposited and returned to the glove box it is placed in the
Sensor Holder/Base plate. The E-ring is stacked on the base and the electrical contacts are fixed
in place. The Adapter plate is stacked on next and the three are bolted together using conflat
seals and standard bolts. Rubber O-rings are laid in the grooves of the Adapter plate with a
minute amount of vacuum grease. The barrier sample is aligned on the interior O-rings and the
Sample Cover is bolted down over it. Proper torque was reached by using a torque screwdriver
and tightening in sequential steps to the target torque. Over tightening of the bolts will cause
sample deformation which could result in barrier failure. Depending on the type of experiment
desired, the correct Sample Cover is chosen. For baseline measurements the solid cover is
used. For a barrier sample the bored sample cover (Figure 3.4) is used. The Shroud is then
bolted in place around Sample Cover. Assembly can be completed in as little as 45 min after
the Ca has been deposited.
Once assembled as shown in Figure 3.7, the apparatus was placed in the environmental
chamber described earlier. The connections are made to the Keithley multimeter and faraday
cage around the meter; data recording is started. It was found to be best practice to give the
apparatus time to reach temperature equilibrium. This was done by setting the initial
![Page 89: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/89.jpg)
77
Figure 3.7 Fully Assembled Ca Test Apparatus
![Page 90: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/90.jpg)
78
conditions within the chamber at 70 °C and 25% humidity for one hour. Maintaining a low
humidity for one hour prevents condensation on the apparatus. If this step is skipped water
will condense along seal on the sample of the surface. After equilibrium is reached conditions
can be set to any desired temperature and humidity.
Our new apparatus has advantages over previously experimental setups. If it is
necessary to separate the WVTR from the oxygen transmission rate (OTR) a special sample
cover can be created with ports. This would allow the experimenter to dope UHP N2 with a
predetermined amount of O2 or H2O over the barrier sample. A measurement conducted in
this way would allow the separation of permeation rates. Also, the seals are reusable for
multiple tests. This decreases the cost of using the apparatus as well as making it
nondestructive. The same barrier sample to be tested repeatedly decreasing the number of
samples needed to get meaningful results. Multiple parallel apparatus’ can be easily tested
simultaneously further increasing throughput.
Results and Discussion This new apparatus can measure very low WVTR values. However, obtaining low WVTR
values requires that residual H2O is removed from the components and surface area in the Ca
test apparatus. The main source of residual H2O is the Viton differential seals. Fortunately, H2O
can be outgassed from the Viton by baking in vacuum for more than 72 hours.89 After removing
the residual H2O, this apparatus has reached WVTR values of 3-5x10-4 g/(m2*day) at elevated
temperature with a metal lid. Conductance values that yield an effective WVTR of 2.55x10-4 are
shown in Figure 3.8. This WVTR value is slightly lower than the baseline of the best
![Page 91: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/91.jpg)
79
48
46
44
42
40
38Co
nd
ucta
nce
(x1
0-3
mh
o)
250200150100500Time (hr)
WVTR = 2.55 x10-4
g/m2/day
110126
70 °C / 28 %RHSteel Cap
Figure 3.8 Baseline Conductance Curve for New Apparatus
![Page 92: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/92.jpg)
80
commercial instruments. However, it has the potential for capabilities that the commercial
instruments do not have, such as the measurement of OTRs and WVTRs independently.
Other virtues of this new Ca test apparatus are that the Ca film can be replaced without
destroying the barrier sample. Retesting the same barrier with different Ca films can narrow
the experimental uncertainty in the WVTR measurement. The WVTR values from the uncoated
polymers appear to show a large lag time resulting from H2O equilibration in the polymer
substrate prior to transmission into the Ca test apparatus. The effect of H2O percen RH on this
lag time is significant. It is important to properly measure this lag time before measuring
barriers. Otherwise, it is impossible to determine whether the WVTR measured is due to the
barrier or polymer lag time if the test is only performed over a period of a few days.
![Page 93: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/93.jpg)
81
Chapter 4 Polymer Substrate Effects
Abstract
Gas diffusion barriers on polymers with water vapor transmission rates (WVTRs) as low
as <10-6 g/(m2*day) are required for organic electronic and thin film photovoltaic devices.
Barrier materials are deposited on flexible polymer substrates and the WVTR of this composite
system is measured. The effects of the polymer substrate must be characterized to understand
the measured WVTRs. The polymer substrate can affect many characteristics of the WVTR
measurement. The polymer can alter the lag time and also influence the water corrosion of the
barrier. In this study, heat stabilized poly(ethylene naphthalate) (PEN) was used as a model
polymer substrate. The Calcium Test using a resistance measurement was used to monitor the
effect of water flux through the polymer as a function of temperature and relative humidity. Ca
sensor lifetimes are inversely proportional to the water vapor flux incident on the PEN polymer
surface. Ca sensor lifetimes showed little temperature dependence. The characteristic form of
the Ca test conductance vs. time curves is examined.
Introduction
Atomic Layer Deposition (ALD) is very effective as a technique to deposit conformal,
transparent, gas diffusion barriers.9, 13, 36 These barriers can protect organic electronic or thin
film solar devices from degradation by water and oxygen.10, 90 Water vapor transmission rates
(WVTRs) of <10-6 g/(m2*day) and oxygen transmission rates (OTRs) at STP of <10-5 cm3/m2/day
are needed for organic based electronics to reach device lifetimes of 10,000 hrs.10 These
requirements arise from the sensitivity of the low work function metals (e.g. Ca, Li, Mg) in these
![Page 94: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/94.jpg)
82
devices. ALD Al2O3 films on polymers are excellent barriers with WVTRs equal to, or better
than, the sensitivity limit of the Ca test 36 ( ≥1 x10-4 g/(m2*day)).
Measurements of WVTRs usually ignore the effect of the polymer substrate because the
WVTR of the polymer is so large at ~1 g/(m2*day). Any saturation behavior or lag times
resulting from the polymer substrate are usually assumed to be negligible. However, the
polymer accounts for a significant fraction of the barrier/polymer system. A typical Al2O3 ALD
barrier is 0.025 µm. A typical PEN polymer thickness is 50-200 µm (Figure 1.9). In addition, the
ALD barrier is usually deposited on only one side of the polymer. As a result of this asymmetry,
the ALD barrier can either face the incident H2O flux or face away from the incident H2O flux.
Figure 1 shows a representative schematic of an Al2O3 ALD barrier on a PEN substrate. The
response to water exposure by the polymer can have multiple effects on a barrier. Swelling
could disrupt a barrier by applying tensile strain. An accumulation of water at the interface
may cause degradation or delamination of the barrier.
Another parameter that is often ignored when measuring WVTRs using the Ca test is the
time for the water flux to saturate the polymer. This saturation time is required before H2O can
diffuse through the polymer at a steady state. This time will be included in the barrier’s
measured lag time by the Ca test. The saturation time will depend critically on whether the
ALD barrier faces the incident H2O flux or faces away from the incident H2O flux. If the water
flux is meeting the barrier first the flux into the polymer will be greatly limited. This will
increase the time it takes to fill any bulk reservoir sites in the polymer. The total lag time is the
sum of the time to saturate the polymer and reach steady state diffusion through the barrier.
![Page 95: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/95.jpg)
83
To understand the times required to saturate the polymer, Ca tests were performed for
the PEN polymer without any ALD barrier. Additional Ca tests were conducted at different
temperatures under constant H2O flux to determine the activation barrier for H2O transport
through the PEN polymer. Further tests were carried out with unsaturated and saturated PEN
to determine the effect of polymer uptake on Ca test performance. After fully understanding
the role of the PEN polymer, we can then return to the ALD barriers on the PEN polymers and
extract meaningful WVTR values. Detailed understanding of the polymer/barrier system should
increase our ability to model such systems.
Electrical Ca Test
The Ca test for these studies was based on changes in the electrical conductance of a Ca
film during oxidation. The calcium test uses a thin, metallic, calcium layer as a sensor for water
and oxygen permeation.9, 12, 13, 16 As oxygen or water permeate the barrier, they react with Ca
to form calcium oxide [CaO] or calcium hydroxide [Ca(OH)2], both of which are electrically
insulating. Other groups have also employed an electrical conductance Ca test.34, 37, 91 In some
electrical conductance Ca test research samples are prepared by depositing Ca metal on a
polymer substrate. Silver contacts were then added over the Ca metal and the sample was
covered with a glass lid using an epoxy seal. One major problem with this set-up is that the
epoxy seal can lead to a high baseline WVTR. Soft epoxies do not provide a sufficient barrier to
water ingress.
The conductance test assumes that uniform Ca oxidation occurs in a top-to-bottom
fashion.34 Since barrier permeation is known to be defect-dominated, uniform Ca oxidation
![Page 96: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/96.jpg)
84
may not be occurring if the Ca film is located close to the barrier. In the case of pinhole defects
in a barrier, the Ca film may be oxidizing in localized areas under the pinhole defects. When
water penetrates a defect it will begin to oxidize the Ca equally in all directions. A hemispherical
oxidation zone will expand from the defect until it reaches the full thickness of the Ca metal.
The zone will them begin to expand as a cylinder under the barrier (Figure 1.8). Depending on
the distribution of defects, large conduction paths can become electrically isolated without
oxidizing all of the Ca metal in the electrical path. Such situations result in a sharp decrease in
conductance resulting from the restricted percolation path rather than true Ca oxidation. This
makes it impossible to determine a WVTR using the standard interpretation of Ca test
conductance curves.
Problems with the Ca Test
There are some limitations of the optical implementation of the Ca test. The largest
limiting factor for the electrical Ca test is also the epoxy edge seal. There are other problems
with the Ca test using the conductance method. The oxidized Ca could be either CaO or
Ca(OH)2. This variance is caused by the reaction sequence that Ca metal undergoes when
exposed to water and oxygen. If Ca metal is exposed to oxygen first, it will form CaO (ΔHfo=-
635.09 kJ/mol). If the CaO is sequentially exposed to H2O will with form Ca(OH)2 (ΔHfo=-
986.09). Since only the first change from metal to oxide (or hydroxide) causes a conductance
change this means the two permeation rates cannot be separated. The typical solution to this
is that all oxidation is assumed to be due to water permeation and an “effective WVTR” is
typically reported. In addition, the gluing of the polymer to the Ca film on the glass substrate
![Page 97: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/97.jpg)
85
using epoxy means that the polymer cannot be reused after the Ca test. Consequently, many
individual samples are required to obtain meaningful results.
The conductance test assumes that uniform Ca oxidation occurs in a top-to-bottom
fashion.34 Since barrier permeation is known to be defect-dominated, uniform Ca oxidation
may not be occurring if the Ca film is located close to the barrier.14, 38, 39 This is the original
configuration that has been widely used. In the case of pinhole defects, the Ca film may be
oxidizing in localized areas under the pinhole defects. Depending on the distribution of defects,
large conduction paths can become electrically isolated without oxidizing all of the Ca metal in
the electrical path. Such situations result in a sharp decrease in conductance resulting from the
restricted percolation path rather than true Ca oxidation. Oxidation via pinholes occurs in a
hemispherical fashion. As long as the radius of the hemisphere is smaller than the thickness of
the Ca film the electrical method provides a meaningful result.
A second problem for the conductance method arises from the metal used to form the
electrical contacts with the Ca metal. Silver and gold are common choices for good electrical
contacts that will not corrode. Unfortunately, both of these metals form crystalline alloys with
Ca at temperatures where the permeation tests are conducted.40, 41 There are multiple alloy
phases that can form, all of which have exothermic enthalpies of formation ranging from -41 to
-106 KJ/mol.42 These alloys are typically studied at elevated temperatures. However, recent
results have shown that annealing at low temperature (270 °C) for as little as 15 minutes can
affect Au-Ca alloy structure.43 This alloy formation leads to changes in the conductance
measurement that cannot be accounted for and increases the uncertainty in the
![Page 98: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/98.jpg)
86
measurements. Other metals besides silver and gold must be employed to avoid this difficulty.
After noticing this problem with gold contacts we determined that Cr metal made an
appropriate electrical contact.
Experimental We used the equation originally published by Paetzold in 2003 with some of our own
modifications.
( )
( )
( )⁄
(4.1)
In Eq. 4.1, P = Permeation Rate (g/(m2*day)); n = stoichiometric coefficient; M(Ca) = Molar
mass of Ca; M(reagent) = Molar mass of H2O or O2; δ = density of Ca; ρ = resistivity of Ca; l =
separation of contacts; b = width of Ca pad; 1/R = Conductance (mho). We added two factors to
the equation they are: the total area of Ca, including that on the electrodes, ACa and the area of
the barrier being measured, Ab. Our additions were necessary to take into account the
difference between the barrier and C areas. In Paetzold’s original test the Ca was deposited and
the barrier directly so the areas were identical.
This model makes a few critical assumptions. First, that Ca corrosion is uniform in one
dimension, perpendicular to the barrier. Secondly, that all corrosion is due to either water or
oxygen. Third, the film is uniform in density and resistivity. The fourth and final assumption is
that the area of the Ca pad and the area of the barrier are equal.
If we examine these assumptions we find a few problems. At first it seems reasonable
that, if the barrier is pinhole free, oxidants permeating the barrier will uniformly diffuse.
![Page 99: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/99.jpg)
87
Barrier permeation is known to be defect-dominated.14, 33 If the barrier is oriented toward the
humid atmosphere the following happens. The oxidant permeates a pinhole and enters the
polymer; the concentration of water expands in all directions equally. This forms a
hemispherical wave that diffuses through the polymer (Figure 1.7). If the separation between
the defects is less than the polymer thickness the hemispheres will join. Once the hemispheres
join, a uniform wave front of water is formed. When this wave front reaches the Ca we would
expect it to also oxidize uniformly. For this to happen all of the defects must have a separation
less than the thickness. The model doesn’t hold true when barrier defects act as point sources.
If the defects have very large separations the hemispheres will reach the Ca at individual points.
The Ca will begin to oxidize at a point. If the Ca is directly deposited on the barrier this effect is
even more pronounced. Without the intervening polymer layer the Ca will oxidize and more
tightly localized points (Figure 1.8). The oxidation will spread in a hemispherical wave front
through the Ca just at is did through the polymer. Once the hemisphere has moved to through
the calcium thickness the oxidation will expand in as a cylinder centered on the defect. As
oxidation progresses the edges of the cylinders will meet. Depending on the distribution of
defects, large conduction paths can become electrically isolated without oxidizing all of the Ca
metal in the electrical path. Such situations result in a sharp decrease in conductance resulting
from the restricted percolation path rather than true Ca oxidation. This makes it impossible to
determine a WVTR using the standard interpretation of Ca test conductance curves.
If the barrier is facing the atmosphere this could take days depending on the defect size
and separation. With the barriers facing the Ca sensor, polymer saturation should happen
![Page 100: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/100.jpg)
88
within a day or two depending on experimental conditions and polymer substrate. Water
absorption by the polymer may lead to barrier disruption if the polymer expands.
The assumption of water being the major oxidant is made because limited results have
shown that the oxidation of the Ca varies greatly with temperature and humidity content. This
has led many to believe that water is the predominant penetrant. This may simply be that the
activation energy need for oxygen to react with a Ca surface is higher than H2O. No apparatus
has yet been built that can separate OTR and WVTR for barrier films. We did not perform these
experiments, but our apparatus could be easily adapted to. For the purposes of our work we
will be report the apparent WVTR for barrier films.
New Ca Test Apparatus
We have developed a conductance Ca test apparatus that does not use an epoxy
adhesive to seal the polymer substrate to the Ca test pad. Instead of an epoxy, a differential
seal is used to attach the polymer substrate and isolate the internal volume of the Ca test
apparatus from the outside. This differential seal prevents H2O ingress and allows the samples
to be removed after the Ca test; overcoming two of the issues with previous Ca tests. The
advantage of our apparatus is the separation of the Ca sensor from the polymer. With a sensor
placed in direct contact with the polymer the oxidation will be more localized near the defects
in the barrier. In our system, the gas volume above the Ca sensor allows water permeating the
barrier an equal probability to impact the entire Ca surface. This should result in oxidation
closer to the uniform oxidation model used by Paetzold. Ideally this should result in a more
accurate WVTR calculation from the conductance slope.
![Page 101: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/101.jpg)
89
We utilized a 4-wire resistance measurement to increase accuracy. Using 4-wire
resistance removes the lead resistance from the circuit. This will cancel minor differences in
lead length and crimped connections. The electrical conductance of the Ca film is monitored
with a Keithley 2700/7700 mainframe and multiplexer combination inside a grounded faraday
cage. To further reduce electrical noise the meter and computer were powered via a line
power conditioner. This instrumentation allows us to run multiple samples in parallel through
the entire experiment. Running multiple tests in parallel helps the user detect problem
samples. It also decreases the time need to obtain meaningful experimental comparisons. The
environmental chamber used was an ESPEC BTL-400. The chamber utilizes a Watlow F4
controller that was linked to LabView using an RS-232 (Modbus-RTU) connection. A custom
LabView program was used to record the sample conductance five times at one minute
intervals for each sample. The measurements were then averaged to attenuate any electrical
noise present in the signal. The same program recorded the temperature and humidity
reported by the Watlow controller at the same interval. As long as the controller is powered
the temperature and humidity are recorded. This is helpful if the humidity chamber were to
enter a “fault” condition and stop maintaining the internal environment.
Calcium sensors were fabricated on microscope glass slides. The slides were immersed
in acetone and sonicated for 15min twice. Next they were washed with, and immersed in,
methanol and sonicated for 15 min. While still submerged in methanol they were placed in a
class 100 particle hood. They were removed from methanol, blow dried with filtered N2 and
masked. The masked slides were attached to a sample platter for placement into a PVD
chamber. Chromium metal was sputtered with RF-Magnetron sputtering onto the masked
![Page 102: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/102.jpg)
90
slides. The sputtering rate was approximately 4.5 Å/s, determined with ex-situ FIB/SEM
measurements. Final Cr thickness was approximately 540 nm. The slides were cut into 1”x 1”
squares. They were cleaned a second time and placed into our glove box. Immediately prior to
Ca test assembly, this Cr and glass sensor substrate was transferred to the PVD chamber using
the attached transfer arm. It was attached to a motorized spindle within the chamber. Once
the chamber was at base pressure the sensor substrate was shield and a 1 minute sputter was
used to remove any CaO from the Ca target surface. The shield was removed and the Ca sensor
film was sputtered onto the Cr/glass sensor substrate. The completed sensor was returned to
the glove box for immediate assembly into the test apparatus.
Polymer samples were created using a custom die to cut circles from a sheet of Teonex
Q65F from Teijin DuPont Films. The polymer sheet was stored in the water/oxygen-free glove
box. A portion was removed from the glove box and a large number samples were cut and
stored for use when needed. The polymer samples are immediately returned to the glove box
and stored until needed.
Results and Discussion The conductance through the Ca sensor film decreases with time as the Ca film is
oxidized by O2 or H2O. As with studies performed by other groups, all Ca oxidation will be
assumed to be due to water. Conductance curves for uncoated PEN polymers show a large
“lag” time. This usually believed to result from the time it takes for H2O to saturate the
polymer substrate and barrier prior to H2O transmission into the Ca test apparatus. Results at
70 °C and 40% RH are shown in Figure 4.1. To ease discussion we will define terms for the
different parts of the typical conductance versus time curve. The “lag region” starts at the
![Page 103: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/103.jpg)
91
Figure 4.1 Bare PEN 70 C / 40% RH
1.0
0.8
0.6
0.4
0.2
0.0
No
rma
lize
d C
on
du
cta
nce
2520151050Time (hr)
70°C / 40% RHBare PEN
111013
"Lag" Region
Knee
Fall Off Region
Sensor Lifetime
End Point
![Page 104: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/104.jpg)
92
beginning of the test and goes until the “knee”. After the knee, the rapid fall off of the
conductance is the “fall off region”. The point at which the conductance reaches zero is the
“end point”. From t = 0 to the end point (conductance <10-5) is the “sensor lifetime”. It is
important to note that regardless of the liftime of the sensor the conductance curve always has the
same characteristic shape. The only change between curves collected under varying conditions and
sample types is the length of the “lag” time.
For the example in Figure 4.1, the conductance initially is nearly constant for the first ~12
hours and then drops suddenly after ~16 hours. The currently accepted interpretation is that
~16 hours is needed for H2O to saturate the PEN polymer prior to H2O transport through the
PEN polymer. H2O transport through the polymer may not be possible until H2O has “titrated”
all the reservoir states. The steady state slope of the conductance after ~16 hours could then
be used to determine a WVTR.
Conductance measurements were performed to determine the sensor lifetime as a
function of relative humidity at 70 °C. These experiments were performed for bare PEN
polymer substrates with no ALD barrier. The results are shown in Figure 3. The effect of H2O %
RH on the Ca film lifetime is significant. A sensor lifetime change of 20 hours can be observed
when the RH is changed from 25% to 80%.
Figure 4.3 shows that the Ca film lifetime is shorter for the higher H2O vapor pressures at
70 °C. This dependence is consistent with a simple mechanism where each H2O collision with
the PEN polymer has a certain probability of transporting H2O into the polymer. The assumed
mechanism is a multi-step process. Once the water impacts the surface is must diffuse into the
![Page 105: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/105.jpg)
93
35
30
25
20
15Se
nso
r L
ife
tim
e (
hr)
3.53.02.52.01.5
1/Flux (10-27
m2s / molec)
Figure 4.2 Ca Film Lifetime vs. 1/Flux
1.0
0.8
0.6
0.4
0.2
0.0
Norm
aliz
ed
Co
nd
ucta
nce
1.0
0.8
0.6
0.4
0.2
0.0
403020100Time (hr)
70°C / 25% RH
70°C / 60% RH
110927
110928
F = 2.61 x1022
molecules/cm2 s
F= 6.27 x1022
molecules/cm2 s
Figure 4.3 Conductance vs. Time for Bare PEN with Changing Flux
![Page 106: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/106.jpg)
94
polymer bulk. Most polymers are expected to have some absorption capacity. After the PEN
polymer is saturated with H2O, it can diffuse through and evaporate from the other side of the
polymer, enter the Ca test apparatus, and oxidize the Ca film. To test this idea, the percent RH
values at 70 °C were converted to an incident H2O flux. The Ca film lifetime should be inversely
proportional to the H2O flux incident on the polymer. Figure 4.2 shows the relationship between
the Ca film lifetime and the inverse of the H2O flux. There is a linear dependence that is
consistent with the simple mechanism. This implies that there is a simple sticking coefficient
for water on Q65F polymer and is not dependent on surface coverage. It also implies that once
a water molecule is adsorbed it has a constant probability to diffuse into the polymer for a
given temperature.
The next step was to examine the temperature dependence of the Ca film lifetime at
constant H2O flux. These measurements gave an insight into the H2O absorption characteristics
of the PEN polymer at different temperatures. They also gave the activation energy for H2O
transport through the PEN polymer. The activation energy was needed to relate accelerated
tests results to normal conditions. A constant flux of 2.9 x1022 molecules/ cm2/s was
maintained by changing temperature and humidity within an environmental chamber. With a
chosen flux, the temperature and humidity conditions were calculated using √ ⁄ .
The temperature changes have a small effect on the desorption rate of water molecules in a
secondary monolayer. This desorption rate is governed by - ⁄ , where = 4
x1015 ML/s.92 The sensor lifetime decreased with increasing temperature at fixed flux (Figure
4.4). The data can be easily fit with an exponential decay equation: ⁄ . Creating an
Arrhenius plot of the data allowed determination of the permeation energy of the PEN.
![Page 107: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/107.jpg)
95
Figure 4.5 ln(1/Sensor Lifetime) vs. 1/Temperature
-4.4
-4.0
-3.6
-3.2
ln (
1/S
en
so
r L
ifetim
e)
3.103.053.002.95
1000/T (K-1
)
Ep = 12.4 kJ/mol
1.0
0.8
0.6
0.4
0.2
0.01.0
0.8
0.6
0.4
0.2
0.0
No
rma
lize
d C
on
du
cta
nce
50403020100Time (hr)
120304
120313
70°C / 28.8 %RH
50°C / 64.6 %RH
F = 2.9 x 1022
molecules/cm2 s
Figure 4.4 Sensor Lifetime vs. Temperature at Constant Flux
![Page 108: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/108.jpg)
96
Normally this would require plotting ln(WVTR) vs. 1/T. However, since it was not possible to
determine an accurate WVTR, another approach was used. Water vapor transmission rates are
proportional to 1/lifetime. Thus, by plotting ln(1/lifetime) vs. 1/T we can determine a
permeation energy. The permeation energy measured in this work is 12.4 kJ/mol (Figure 4.5).
This is given as an upper limit and is congruent with values reported for other polymers.93-95
An important factor in using polymer substrates is their ability to absorb water. The
amount of water that the polymer can absorb will change the observed lag time for a barrier.
This may extend the lag time beyond the test duration; particularly when using short,
accelerated tests under harsh conditions. Changes in the polymer structure due to water
content (such as swelling) may also adversely affect barrier coatings in unforeseen ways.
We applied a simple mental model to the process of water diffusion through a polymer
with a reservoir (Figure 4.6). When a water molecule adsorbs onto a polymer surface (and
doesn’t immediately evaporate) it will have some residence time where it may migrate. There
is a potential for it to gain enough energy to either evaporate or penetrate the polymer. We
are interested in the penetration case. If the polymer contains reservoir sites the water will
have some equilibrium between being bound the sites and diffusing through the bulk polymer.
When the amount of water is much less than the number of sites the water will have a higher
probability to move from site to site and remain localized. Once the sites have been saturated
incoming water will result in molecules being forced out. Some of them will move to the sensor
side of the polymer where they can evaporate. Once they have evaporated they are free to
diffuse to the sensor and react, causing a change in conductance.
![Page 109: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/109.jpg)
97
Figure 4.6 Water Permeation Through Saturated and Dry Polymers
Figure 4.7 Sensor Lifetime vs. percent RH for Dry and Saturated PEN
40
30
20
10
0
Se
nso
r L
ife
tim
e (
hr)
807060504030
Humidity (%RH)
Dry H2O Saturated
![Page 110: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/110.jpg)
98
To explore the reservoir effect of the PEN polymer, both dry and water-saturated PEN
substrates were tested. The sensor lifetimes were recorded against changes in flux at 70 °C.
The relative humidity was varied from 25% to 80% which were the upper and lower limits of the
humidity chamber. This allowed us to test the dry and saturated PEN substrates between
“normal” and “harsh” conditions. There was no observable difference between using a dry or
saturated polymer substrate (Figure 4.7). This implies that there is little to no reservoir with the
PEN polymer being used.
This result is contrary to the typical interpretation of the “lag” region observed in an
electrical Ca test. If there is no reservoir present, then the question becomes: what causes this
delay in conductance change? We devised a way to test the response of the electrical Ca test
without measuring changes due to the polymer. We simply removed the polymer from the test
apparatus and measured the conductance as usual. The Ca sensor was exposed to our
environmental chamber with no polymer or barrier. The test was conducted at 70 °C and 25%
relative humidity. The low humidity was chosen to extend the life of the Ca metal for as long as
possible. We encountered an unusual response, shown in Figure 4.8. This experiment was
conducted multiple times, each iteration showed the same response.
The conductance shows the same behavior whether there is no polymer, a bare
polymer, or a barrier on a polymer. It is just the “lag” time that increases. The sensor lifetime
measured when no polymer or barrier was present was approximately 9 minutes (Figure 4.8).
However, the first six minutes showed very little change in conductance. This shows that Ca
![Page 111: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/111.jpg)
99
Figure 4.8 Conductance vs. Time for Ca Film Exposed to Atmosphere
1.0
0.8
0.6
0.4
0.2
0.0Norm
aliz
ed C
ond
ucta
nce
12840Time (min)
No Polymer Film70°C / 25% RH567 nm Ca
120222
![Page 112: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/112.jpg)
100
metal conductance does not respond linearly to oxidation as was previously assumed. If Ca
metal thin films showed a linear change in conductance with oxidation we would expect a
straight line. The conductance should show a straight line from initial conductance at t = 0 to
zero conductance at the endpoint. Without a linear response, one cannot calculate an
accurate WVTR from the slope of the graph at any given point with certainty.
Conclusions The polymer substrate can influence the measurement of the WVTR for a gas diffusion
barrier on a polymer. The effects of the polymer substrate have been measured by
determining the C a film lifetime during the conductance Ca test. Ca sensor lifetime is inversely
proportional to incident water flux on the polymer surface. This dependence is expected if
each H2O collision with the polymer surface has a constant probability of being transported into
the polymer. Water permeation showed little temperature dependence at constant incident
H2O flux. Permeation energy of 12.4 kJ/mol was measured for PEN. Ca tests performed with the
sensor open to the humidity chamber environment showed a non-linear response to oxidation.
This calls into question the accuracy of WVTRs obtained using the electrical Ca test. More
studies are needed to establish how the conductance of Ca metal thin films changes with
thickness and oxidation.
![Page 113: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/113.jpg)
101
Chapter 5 Mechanical Testing of ALD ZnO
Abstract There is great interest in creating thin, flexible electronics based on organic molecules.
Flexible thin film devices require materials that can withstand repeated stress and strain
loading while maintaining electrical perfromance. Measuring the critical strain of ultrathin ALD
films is difficult with currently available methods. We have successfully measured the critical
strain of a range of thicknesses of ALD ZnO films using both 4-point probe and CLSM methods.
Both methods showed limitations for thinner films (<40nm) and cannot be used to reliably
measure films below that threshold. The critical strain of 22nm-132nm ALD ZnO on
200micrometer PEN was determined to be between 1.1% and 0.65%. This strain is too low for
flexible barrier applications which require 3-5% critical strain. We have shown that thin
(<100nm) ALD ZnO films are not flexible enough for flexible conducting oxide/barrier
applications. We have also shown that ALD ZnO films seem to follow current fracture models
which predict that crack density decreases as film thickness increases.
Introduction There is great interest in creating thin, flexible electronics based on organic molecules.
This is made possible by creating the devices on a polymer substrate. For flexible electronics
both good flexible water and oxygen gas barriers and flexible transparent conducting oxides are
required. A typical polymer has a water vapor transmission rate (WVTR) on the order of 0.1-10
g/(m2*day).15 The transmission of such a large quantity of water vapor through the polymer
into the organic electronics results in failure of the device. Atomic layer deposition (ALD)
provides an effective solution to this problem since ALD is capable of coating water vapor
![Page 114: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/114.jpg)
102
barriers onto devices of any geometry with a conformal film of precisely controlled thickness.
Aluminum oxide (Al2O3) ALD films of ≥12nm have been shown as diffusion barriers with a WVTR
(~10-4 g/(m2*day)) that is much lower than just the polymer and may be low enough to protect
some water-sensitive devices.9, 11, 13 However, in order to make flexible organic electronics a
reality, flexible diffusion barriers are not the only advancement that is needed. It is also
necessary to create a flexible electrode capable of withstanding day-to-day use while
maintaining steady electrical characteristics. ALD might also provide a solution to this problem
as nanometer thin films are more flexible than thicker films. Indium tin oxide (ITO) is the most
widely used transparent conducting oxide (TCO) because of its favorable electrical
characteristics and high transparency in the visible range.96, 4 The main disadvantage of ITO is its
high cost due to the rarity of indium. Also, indium migrates in devices from the ITO electrode to
the organic film which can decrease device efficiency. It is therefore of great interest to find a
cheaper alternative TCOs that is also flexible.96-98
When a material is flexed, the surface farthest from the center of curvature is put into
tensile strain and the inner surface undergoes compressive strain (Figure 1.3 and Figure 1.2).27
This results in the formation of a neutral plane within the material which sees no strain. If the
material is uniform, i.e. an uncoated polymer, the neutral plane exists in the center of the
material. As coatings are added, the neutral plane shifts towards the face where the coating
was applied. ALD coatings are typically three orders of magnitude thinner than the polymer
substrate (or device) and the neutral plane remains relatively unchanged. Linear tensile strain
is described by
, where L is the original sample length. In a bent polymer a gradient that
![Page 115: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/115.jpg)
103
Figure 5.1 Instron Polymer Flexion Adaptor
![Page 116: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/116.jpg)
104
exists as shown in Figure 1b. The strain is obtained through
, where y is the distance
from the neutral plane and R is the radius of curvature.12 The strain at the surface of the
substrate is taken to be the strain through the ALD coating since any gradient that exists within
the coating would be negligible. This relationship gives the strain applied to an ALD film,
,
where T is the thickness of the substrate.
As a coated sample is bent, the strain continues to increase until such point that the
coating will fracture. The strain at which this occurs is known as the critical strain (εc) and is
usually believed to be proportional to the reciprocal square root of the film thickness.30 Initial
cracks will lengthen and additional fractures will occur if the increase in strain continues until
the number of fractures reaches saturation.28 The failure mechanism for thin brittle layers is
different from that of bulk materials. In bulk materials, a crack, once initiated, will propagate
the full width across the material. For thin films, cracks initiate at point defects and propagate
to a finite length for a given strain. As strain increases, the crack length will increase
proportionally until either the maximum stable crack length ( ) or critical crack propagation
strain ( ) is reached. Once one of these conditions is met the crack will propagate to the full
width of the film.29
We designed a mechanical adaptor for an Instron Universal Testing Machine (Model
5565) that flexes the polymer samples in a controlled manner (Figure 5.1). The Instron testing
machine uses a linear actuator to close the distance between the adaptors causing curvature of
the film. Depending on the physical orientation of the film when placed in the adaptors, the
ALD coating can be placed under tensile or compressive strain and flexed repeatedly to a
![Page 117: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/117.jpg)
105
specified radius of curvature that corresponds to the desired applied strain. The method also
has great sensitivity due to the instrument’s translational resolution of 50µm.
Zinc oxide (ZnO) ALD is known to be polycrystalline99. The small cracks that form around
defects in coatings at very low strains29 would not necessarily lead to an increase in resistance if
present in a conductive film but do provide nuclei for larger cracks to begin once the film is
strained. Previous research has used ALD to create ZnO/Al2O3 alloy films that showed changes
in the conductivity possibly due to influence on the crystal structure of the ZnO.99, 100 Doping of
ZnO films with other metals, such as aluminum, leads to a decrease in their crystallinity. If ZnO
alloys are to replace ITO as the anode of choice for flexible organic electronics, we need to
understand their performance under strain.
In order to explore these properties of a thin film it is necessary to have a sensitive
technique to monitor changes in the film’s behavior. The cracks that occur in film may, initially,
be very small in comparison to the film thickness. To determine an accurate measurement of
the critical strain, we must be able to detect these minute changes as soon as they occur during
testing. Depending on the properties of the film, i.e. conductivity, there are few methods that
can be used. Cracking in thin Indium tin oxide (ITO) films has been studied with sensitive
resistance measurements. We applied a similar method to explore cracking of ALD ZnO films
which exhibit similar electrical properties to ITO.
Experimental Critical tensile strains of ALD ZnO films were determined through two different
methods. The initial work used a 4-point probe measurement to see resistance changes due to
![Page 118: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/118.jpg)
106
cracking whilst the second method used Confocal Microscopy (CM) to image and measure the
cracking of the ZnO films optically.
Four Point Probe
Polymer substrates, 1” x 3”, were cut from 75µm Kapton® (DuPont) or 200µm PEN
(Teijin Films). The choice of substrate was based on the strain the films were to be bent to as
PEN can withstand higher strains but Kapton afforded higher strain resolution at lower range of
applied strains. The substrates were rinsed with DI water, methanol and blow dried with UHP
Nitrogen under a class 100 particle hood. They were then attached to 1”x3” clean glass slides
at each end with 3M™ High Temperature Aluminum Foil Tape 433. Twelve samples were loaded
into a viscous flow ALD reactor for each thickness.
Confocal Microscopy
Polymer substrates, 4cm by 1cm, (200µm thick PEN, Teijin Films) were rinsed with DI
water, then 100% ethanol and dried using UHP Nitrogen. Resulting substrates were attached to
a 4” by 4” clean glass slide at each end by 3M™ High Temperature Aluminum Foil Tape 433, 8
PEN strips to one glass slide. Up to 3 glass slides (24 samples) were loaded in the ALD reactor
for each thickness.
ZnO Deposition
All ALD depositions were performed using a viscous flow ALD reactor (described
elsewhere) at 120 °C.9 A seed layer of 50 cycles of ALD Al2O3 using TMA (Sigma-Aldrich) and
water (Fisher HPLC-grade) was grown on the polymer. The seed layer was used to ensure
consistent nucleation of ZnO across the polymer. The ZnO deposition began immediately after
![Page 119: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/119.jpg)
107
the Al2O3 deposition was complete without exposure to atmosphere. Different thicknesses of
ALD ZnO were deposited using DEZ (Sigma-Aldrich) and water (Fisher HPLC-grade).
Strain Application
All samples were repeatedly bent (10 times) to the desired strains using an Instron
Universal Testing Machine, Model 5565 (Figure 5.2). Plate separation was measured manually
on every cycle using Mitutoyo Absolute Digimatic calipers. Strains were calculated using the
approximation that the film bend follows half the circumference of a circle of radius r where 2r
= plate separation. The variation in measured plate separation yielded error bars of +/- one
standard deviation.
For the 4-point probe portion of the study, a series of 3 samples were selected from each
thickness batch. They were selected based on the consistency of the initial resistivity measured
over the entire film. Samples that showed large variations were not used. This was done so
that apparent resistivity changes in the film could be attributed to applied strains and not
coating variations. Since the 4-point probe is a non-destructive and non-contaminating
method, the samples were bent and then measured before the next, slightly higher, strain was
applied. By doing this we were able to consecutively bend the samples through the strain
series. The nature of the Confocal Microscopy (CM) method did not allow this sequential
straining of one given sample.
After the CM samples had been bent to the desired strain they were carefully transferred to 1”
by 3” glass slides (2 samples to a slide) and were fixed in place using clear nail varnish. Samples
were then imaged using confocal microscopy. Images were collected using Zeiss’s Zen software
![Page 120: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/120.jpg)
108
Figure 5.2 Polymer Samples in Flexion Adapter
![Page 121: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/121.jpg)
109
to control a Zeiss LSM 510 Meta confocal system with a 100x objective, 1.40 NA (Carl Zeiss,
Germany) (pixel size at 500x = 0.18 µm/pixel). Images were later processes in ImageJ to convert
.LSM files to .tif files which were later edited in Picasa3 to optimize image contrast for crack
counting. Cracks were counted manually. For a given thickness and strain 3 samples were
grown simultaneously which were subsequently strained and imaged together. 3-5 confocal
microscopy images of each of these 3 samples were taken and analyzed to give the error bars of
+/- 1 standard deviation.
Results and Discussion We utilized a Signatone S-3001-6 four-point probe base with a Signatone SP4-40045TFS
head. A Keithley 487 Current Source and Keithley 2400 DMM connected to a computer to
measure the resistivity of the films. Using the 487 and 2400 made it possible to use a larger
range of currents. A LabView VI was used to control the instruments and record the I-V curves.
The probe separation of one millimeter allowed us to examine a small portion of the film at a
time. Multiple readings over a small area were averaged to remove any changes in contact
resistance between the probes and different film points. Before the film had been strained this
measurement was directly converted to the resistivity of the film. After the films had been
strained and began to crack, the I-V characteristics of the film were recorded by the computer
as a change. This is due to the changes in path the current must take. There are three possible
physical changes that affect an I-V curve. The first possibility is the formation of a crack that
penetrates the full depth of the ALD film with the crack walls separated by enough distance to
prevent conduction. This will result in the current taking a longer path to flow around the crack.
The second possible occurrence is related the first because our samples are flexed and then
![Page 122: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/122.jpg)
110
returned to a flat position for testing. I t is possible that a crack that penetrates the film
thickness under flexion returns to a “closed” position when the substrate is flattened. This will
result in a contact resistance between the sides of the crack, which, if large enough, should be
detectable by a four-point probe. The third is a crack that penetrates to a partial depth of the
film,101 decreasing the amount of material available for conduction. The values measured after
these changes are not the true resistivity but what we will call the “apparent resistivity”. The
change in name is important because resistivity is an inherent property of the unbroken film
and cannot be changed by cracking. However, if one were to take a film with an unknown
flexion history and apply the same four-point probe measurement process, the result would be
the “apparent resistivity”. In Figure 5.3 the apparent resistivity vs. percent strain has been
plotted for three 44nm ZnO ALD films. The values are constant for the first portion of the
curve, 0-0.75% strain. This is the true resistivity of the film. At slightly less than 1% the films
begin a very sharp increase in apparent resistivity. The point where this change begins to occur
is the critical strain (εc). The number of cracks and their length continues to increase with
increasing strain until the number of cracks has reached a saturation point.30 This is seen as a
leveling out of the apparent resistivity curve at higher strains shown in Figure 5.3. The four-
point probe’s ability to see these small changes provides us with a powerful tool to examine
very thin films, however, measurements of films below 44nm proved difficult. The four-point
probe is equally sensitive for much thicker films. This gives us a fairly large range of film
thickness to investigate using a single technique. For our 100nm samples, shown in Figure 5.4,
we can see that they behave very consistently in the early portion of the strain curve. They also
show a very consistent critical strain. However, after the critical strain the behavior becomes
![Page 123: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/123.jpg)
111
120
100
80
60
40
20
Avg
. App
aren
t Res
isiv
ity (
x10
-3
*cm
)
2.01.51.00.50.0
% StrainFigure 5.4 Avg. Apparent Resistivity vs. % Strain, 100 nm ZnO
14
12
10
8
6
4
2
Avg
. A
pp
are
nt
Re
sis
tivity (
x1
0-3
cm
)
2.52.01.51.00.50.0
% Strain
Figure 5.3 Avg. Apparent Resistivity vs. Percent Strain, 44nm ZnO
![Page 124: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/124.jpg)
112
much more variable. This could be due to the fracture models that we described earlier. The
disparate film behavior may be due to cracks closing once the film is flattened. It is interesting
to note that the values at the highest strain a very close for all three films. Strains were not
continued past this point since our interest was in the critical strain. The thicker films, 100 and
132nm, showed an interesting artifact between approximately 1.0-1.75% strains. As can be
seen in Figure 5.3, the apparent resistivity values seem to be fairly level compared to the
increase seen after the critical strain. The values then increase rapidly after 2% strain. This can
be seen more clearly in the 132nm films (Figure 5.5). The apparent resistivity stays level
between 1.25% and 1.75% strains. It increases drastically when the films are strains to 2%. This
implies that a second critical strain may exist for the thicker films. This would be consistent
with the partial fracture model described earlier. Since this behavior is not present in the
thinner films, it suggests that the fracture type may depend on film thickness.
In an effort to determine whether or not thin films adhere to the critical strain model:
⁄ we measured the critical strain over a range of thicknesses using 4-point probe.30
The results are shown in Figure 5.6. It can be seen that there isn’t much difference in the
measured critical strains over the thickness range we examined. Each point shown is the result
of six to nine films coated at different times. There was very little deviation in the critical
strains measured for a given thickness. The lowest thickness was restricted by the inability of
our 4-point probe to consistently measure resistivity of films thinner than ~44nm. Films thicker
than 130nm were not measured since such films are over an order of magnitude thicker than a
very good ALD Al2O3 barrier. As these results show no change in critical strain with change in
![Page 125: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/125.jpg)
113
0.14
0.12
0.10
0.08
0.06
0.04
0.02
Avg
. A
pp
are
nt
Re
sis
tivity (
*cm
)
2.01.51.00.50.0
% Strain
Figure 5.5 Apparent Resistivity vs. % Strain for 132nm ZnO ALD
1.2
1.0
0.8
0.6
0.4
0.2
Critica
l %
Str
ain
12008004000
ZnO ALD Thickness (Å)
Figure 5.6 Critical Strain vs. Thickness for 4-Point Probe Method
![Page 126: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/126.jpg)
114
thickness, we decided to measure the critical strain of thinner films (<42nm) using CM. This is
will be discussed later.
Crack Mapping It was of interest to see if cracks in an ALD film could be spatially mapped and related to the
strains that had been applied. Samples were firsts strained to the lowest strain (largest radius of
curvature, largest plate separation). The resistivity of the samples was then measured and the samples
were then strained to the next highest strain and measured again. This was repeated stepwise until the
samples had been strained to the highest the highest strain. As we bend our films between to plates,
the bent films follow an almost uniform curvature. When we bend a sample, the maximum width of the
cracked region is only equivalent to ½ the circumference of a circle with diameter of plate separation.
Since this diameter decreases as we take a given sample through from low strain to high strain, a strain
history is imparted into the film. This is seen with the four point probe as the highest resistivity (due to
highest crack density) in the center of the sample where that section saw the highest strain we went to.
The resistivity decreases as you move further away from that point through regions of the film that saw
less than the maximum strain. We created 132nm samples on Kapton® in an effort to map the strain
history. The ideal strain history is shown in the top image of Figure 5.7. Using the grid shown, where
the black squares are test points, we measured the apparent resistivity at each point. The values
obtained were then mapped out and compared to the curve shown in Figure 5.5. Using the curve we
were able to convert resistivity into a percent stain. The result is shown in the bottom of Figure 5.7. We
obtained good agreement with our ideal model. The resistivity data was also plotted versus position. A
3D surface was interpolated between the points using Igor Pro software. An isometric view of the
surface that was created is shown in Figure 5.8. We can see that while the peak of the resistivity is off
center, the surface has the shape one would expect. These results were very encouraging and we
![Page 127: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/127.jpg)
115
Figure 5.8 Resistivity vs. Position Plotted in 3-D for 132nm ZnO
Figure 5.7 Four-Point Probe Crack Mapping
![Page 128: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/128.jpg)
116
decided to switch methods in order to measure thinner films. Since we were unable to reliably measure
the resistivity of films thinner than 44nm we employed Confocal Laser Scanning Microscopy (CLSM).
Confocal Microscopy
Measuring the cracking of films with CLSM required new samples to be grown and
analyzed. Images were taken of a 90 by 90 micrometer section of the stressed sample surface
and the number of visible cracks was counted. The number of cracks was then plotted as a
linear crack density (cracks /cm versus applied strain). This method worked very well for the
thicker films, and higher strains (Figure 5.9). However, as the crack density decreases it
becomes more difficult to locate and count the cracks. At the high magnifications used it can
be very difficult to locate cracks if there are very few cracks in the field of view. At lower
magnification, the cracks are so narrow that they cannot be seen and thus cannot be counted.
Further difficulties are introduced by scratches on the polymer. It can sometimes be difficult to
differentiate from cracks in the ZnO if they appear in the same orientation as the cracks. We
found that we could destinguish cracks from scratches as cracks came into focus first upon
approaching the surface, whilst scraches only showed up when focusing on the ZnO-substrate
interface beneath the surface. We did this by moving the focal plane from above the sample,
through the ZnO and partly through the polymer untill even the scratches were out of focus and
we were focusing on the interior of the polymer. Almost all the films tested by confocal
microscopy had a determined critical strain of around 1.1%.. As cracks were harder to detect
for thinner films and for strains around that of, or lower than. the suspected critical strain (from
4-point probe measurements), we propose that the actual critical strains of the films are slightly
lower than 1.1%. At strains of around 0.8-1.1% it is likely that cracks were there but could not
![Page 129: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/129.jpg)
117
Figure 5.9 CLSM image of ZnO surface
5
4
3
2
1
0
Cra
ck D
ensity /10
00 c
m-1
)
2.01.51.00.50.0
% Strain
5
4
3
2
1
0
Cra
ck D
en
sity /
10
00
cm
-1)
2.01.51.00.50.0
% Strain
Figure 5.10 Crack Density vs. % Strain for 22nm and 44nm ZnO
![Page 130: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/130.jpg)
118
be found and imaged using confocal micsocopy. Figure 5.10, shows crack density versus applied
strain for a 22nm thick ZnO film on 200micrometre PEN. From the trend in data one may inferr
that data points at 0.95% and 1.1% are not reliable and that there were cracks but they could
not be seen and were thus not recorded, i.e. actual crack density for these points may not equal
0.
Both the confocal and 4-point probe methods were used for several samples of the
same thicknesses. The critical strains obtained for these samples somewhat agree with each
other, showing that these methods give comparable results (Figure 5.11). The confocal
microscopy method gave critical strains of 1.1% where as the four-point probe method gave
critical strains of 0.75-0.95%. The best agreement between the two methods is for the largest
thicknesswhere both methods show a critical strain of 0.95% for films around 100nm. In
general, the critical tensile strains determined from the two methods seem to agree. The trend
of slightly increasing critical strain as film thickness decreases (Figure 5.11) is to be expected, but
the scatter in our results suggests that our observation of this trend may be insignificant. There
is yet to be a reliable, accurate method for determining critical strain in such thin ZnO films
(<42nm). Further corroboration that the CLSM method has some credibility is seen when the
crack density is plotted versus thickness (Figure 5.12).
The curves shown are the crack densities calculated from the confocal method for each
thickness bent to 2.4% and 1.3% strain. The decreasing crack density with increasing ZnO
thickness fits thin film cracking models in the literature.30, 102 This suggests that although the
![Page 131: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/131.jpg)
119
4.0
3.5
3.0
2.5
2.0
1.5
1.0
Cra
ck D
ensity (
x10
3 c
m-1
)
908070605040302010
Thickness (nm)
2.4% Strain 1.3% Strain
Figure 5.12 Crack Density vs. Thickness
1.2
1.0
0.8
0.6
0.4
0.2
Critical %
Str
ain
12008004000
ZnO ALD Thickness (Å)
4-Point Probe CFM
Figure 5.11 CFM and 4-Point Probe comparison
![Page 132: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/132.jpg)
120
determinations of the critical strains using the confocal method are deemed to be not accurate,
the raw data from images where we can clearly see the cracks is reliable.
Conclusions Measuring the critical strain of ultrathin ALD ZnO films is difficult with currently
available methods. We have successfully measured the critical strain of a range of thicknesses
of ALD ZnO films using both 4-point probe and CLSM methods. However, both methods are
limited by film thickness and thinner films (<40nm) cannot be reliable measure with these
techniques. The critical strain of 22nm-132nm ALD ZnO on 200micrometer PEN was
determined to be between 1.1% and 0.65%. This strain is too low for flexible barrier
applications which require 3-5% critical strain. We have shown that thin (<100nm) ALD ZnO
films are not flexible enough for flexible conducting oxide/barrier applications. We have also
shown that ALD ZnO films seem to follow current fracture models which predict that crack
density decreases as film thickness increases.
![Page 133: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/133.jpg)
121
Chapter 6 Conclusions
Ca films were employed to evaluate gas diffusion barriers grown using Al2O3 atomic
layer deposition (ALD). The Al2O3 ALD barriers were grown directly on Ca films. The oxidation
of the Ca films was then monitored by measuring the electrical conductance of the Ca film or by
recording the photographic image of the Ca film. The photographic images revealed that the
Al2O3 ALD films have a small number of pinhole defects. These pinhole defects produce Ca film
oxidation areas that grow radially around the pinhole defect versus time. These pinhole defects
are probably caused by particles on the initial Ca film. The photographic images also observed
a burst of new pinhole defects that appeared suddenly at later times. These pinhole defects
also led to Ca film oxidation areas that grew radially versus time. This rapid “blooming”
suggests that these defects have an origin that is dependent on the Al2O3 ALD film. These
defects may be caused by water corrosion of the Al2O3 ALD films.
The electrical conductance of the Ca film initially showed little change versus time. The
correlation between the photographic images and the electrical conductance then showed that
the conductance dropped when the pinhole defects started to become apparent in the
photographic images. The conductance measurements yielded a WVTR value of ~1x 10-3
g/(m2*day) prior to the appearance of the pinhole defects. There was approximate agreement
between the WVTR values obtained from the electrical conductance and the photographic
images until the rapid “blooming” of new pinhole defects. WVTR values were also estimated
from the time required for the electrical conductance to reach zero. These estimated WVTR
![Page 134: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/134.jpg)
122
values were much higher and indicated that there is much uncertainty in the various
approaches employed to derive WVTRs using the Ca test.
After removing the residual H2O from seals and walls, our Ca test apparatus has reached
WVTR values of 3-5x10-4 g/(m2*day) at elevated temperature with a metal lid using a modified
version of Paetzold’s equation. This WVTR range is slightly lower than the baseline of the best
commercial instruments. Given the non-linear response of the conductance of a Ca film during
oxidation the accuracy of this value cannot be determined satisfactorily. The sensor lifetime
can be used to effectively study substrate materials. The instrument also has the potential for
capabilities that the commercial instruments do not have, such as the measurement of OTRs
and WVTRs independently. The Ca film can be replaced without destroying the barrier sample.
Retesting the same barrier with different Ca films can narrow the experimental uncertainty in
the WVTR measurement. The WVTR values from the uncoated polymers appeared to show a
large “lag” time. The effect of percent RH on this “lag” time is significant.
The polymer substrate can affect many characteristics of the WVTR measurement. In
this study, heat stabilized poly(ethylene naphthalate) (PEN) was used as a model polymer
substrate. The Ca Test using a 4-wire resistance measurement was successfully used to monitor
the effect of water flux through the polymer as a function of temperature and relative
humidity. Due to the inhomogeneity of Ca degradation, sensor lifetime and not WVTR was
used to evaluate bare PEN sheets. Ca sensor lifetimes are inversely proportional to the water
vapor flux incident on the PEN polymer surface. Ca sensor lifetimes showed little temperature
dependence. The characteristic form of the Ca test conductance vs. time curve remained the
![Page 135: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/135.jpg)
123
same for each phase of testing. For coated PEN, bare PEN or atmospheric exposure the Ca
conductance showed the same non-linear response.
Measuring the critical strain of ultrathin ALD films is difficult with currently available
methods. We have measured the critical strain of a range of thicknesses of ALD ZnO films using
both 4-point probe and CLSM methods. However, both methods are limited by film thickness
and thinner films (<40nm) cannot be reliably measured with these techniques. The critical
strain of 22nm-132nm ALD ZnO on 200 µm PEN was determined to be between 0.65% and
1.1%. This strain is too low for flexible barrier applications which require 3-5% critical strain. We
have shown that thin (<100nm) ALD ZnO films are not flexible enough for flexible conducting
oxide/barrier applications. We have also shown that ALD ZnO films seem to follow current
fracture models which predict that crack density decreases as film thickness increases.
![Page 136: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/136.jpg)
124
Bibliography 1. George, S. M., Atomic Layer Deposition: An Overview. Chemical Reviews 2009, 110 (1), 111-131. 2. Ott, A. W.; Klaus, J. W.; Johnson, J. M.; George, S. M., Al2O3 thin film growth on Si(100) using binary reaction sequence chemistry. Thin Solid Films 1997, 292 (1-2), 135-144. 3. Dillon, A. C.; Ott, A. W.; Way, J. D.; George, S. M., Surface chemistry of Al2O3 deposition using Al(CH3)3 and H2O in a binary reaction sequence. Surface Science 1995, 322 (1-3), 230-242. 4. Wilson, C. A.; Grubbs, R. K.; George, S. M., Nucleation and Growth during Al2O3 Atomic Layer Deposition on Polymers. Chem. Mater. 2005, 17 (23), 5625-5634. 5. Goodman, C. H. L.; Pessa, M. V., Atomic layer epitaxy. Journal of Applied Physics 1986, 60 (3), R65-R82. 6. George, S. M.; Ott, A. W.; Klaus, J. W., Surface Chemistry for Atomic Layer Growth. J. Phys. Chem. 1996, 100 (31), 13121-13131. 7. Puurunen, R. L., Surface chemistry of atomic layer deposition: A case study for the trimethylaluminum/water process. Journal of Applied Physics 2005, 97 (12), 121301-52. 8. Suntola, T., Atomic layer epitaxy. Thin Solid Films 1992, 216 (1), 84-89. 9. Groner, M. D.; George, S. M.; McLean, R. S.; Carcia, P. F., Gas diffusion barriers on polymers using Al2O3 atomic layer deposition. Applied Physics Letters 2006, 88 (5), 051907. 10. Lewis, J. S.; Weaver, M. S., Thin-film permeation-barrier technology for flexible organic light-emitting devices. Journal of Selected Topics in Quantum Electronics 2004, 10 (1), 45-57. 11. Potscavage, W. J.; Yoo, S.; Domercq, B.; Kippelen, B., Encapsulation of pentacene/C60 organic solar cells with Al2O3 deposited by atomic layer deposition. Applied Physics Letters 2007, 90 (25), 253511-3. 12. Chen, T. N.; Wuu, D. S.; Wu, C. C.; Chiang, C. C.; Chen, Y. P.; Horng, R. H., High-performance transparent barrier films of SiOx/SiNx stacks on flexible polymer substrates. Journal of the Electrochemical Society 2006, 153 (10), F244-F248. 13. Carcia, P. F.; McLean, R. S.; Reilly, M. H.; Groner, M. D.; George, S. M., Ca test of Al2O3 gas diffusion barriers grown by atomic layer deposition on polymers. Applied Physics Letters 2006, 89 (3), 031915-3. 14. Graff, G. L.; Williford, R. E.; Burrows, P. E., Mechanisms of vapor permeation through multilayer barrier films: Lag time versus equilibrium permeation. Journal of Applied Physics 2004, 96 (4), 1840-1849. 15. Weaver, M. S.; Michalski, L. A.; Rajan, K.; Rothman, M. A.; Silvernail, J. A.; Brown, J. J.; Burrows, P. E.; Graff, G. L.; Gross, M. E.; Martin, P. M.; Hall, M.; Mast, E.; Bonham, C.; Bennett, W.; Zumhoff, M., Organic light-emitting devices with extended operating lifetimes on plastic substrates. Applied Physics Letters 2002, 81 (16), 2929-2931. 16. Kumar, R. S.; Auch, M.; Ou, E.; Ewald, G.; Jin, C. S., Low moisture permeation measurement through polymer substrates for organic light emitting devices. Thin Solid Films 2002, 417 (1-2), 120-126. 17. Tang, C. W.; VanSlyke, S. A., Organic electroluminescent diodes. Applied Physics Letters 1987, 51 (12), 913-915. 18. Burrows, P. E.; Bulovic, V.; Forrest, S. R.; Sapochak, L. S.; McCarty, D. M.; Thompson, M. E., Reliability and degradation of organic light emitting devices. Applied Physics Letters 1994, 65 (23), 2922-2924. 19. Rossi, G.; Nulman, M., Effect of local flaws in polymeric permeation reducing barriers. Journal of Applied Physics 1993, 74 (9), 5471-5475. 20. Chatham, H., Oxygen diffusion barrier properties of transparent oxide coatings on polymeric substrates. Surface and Coatings Technology 1996, 78 (1-3), 1-9.
![Page 137: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/137.jpg)
125
21. Barthelat, F.; Tang, H.; Zavattieri, P. D.; Li, C. M.; Espinosa, H. D., On the mechanics of mother-of-pearl: A key feature in the material hierarchical structure. Journal of the Mechanics and Physics of Solids 2007, 55 (2), 306-337. 22. Mayer, G., Rigid Biological Systems as Models for Synthetic Composites. Science 2005, 310 (5751), 1144-1147. 23. Yeom, B.; Kim, S.; Cho, J.; Hahn, J.; Char, K., Effect of Interfacial Adhesion on the Mechanical Properties of Organic/Inorganic Hybrid Nanolaminates. The Journal of Adhesion 2006, 82 (5), 447 - 468. 24. Du, Y.; George, S. M., Molecular Layer Deposition of Nylon 66 Films Examined Using in Situ FTIR Spectroscopy. J. Phys. Chem. C 2007, 111 (24), 8509-8517. 25. Adamczyk, N. M.; Dameron, A. A.; George, S. M., Molecular Layer Deposition of Poly(p-phenylene terephthalamide) Films Using Terephthaloyl Chloride and p-Phenylenediamine. Langmuir 2008, 24 (5), 2081-2089. 26. Dameron, A. A.; Seghete, D.; Burton, B. B.; Davidson, S. D.; Cavanagh, A. S.; Bertrand, J. A.; George, S. M., Molecular Layer Deposition of Alucone Polymer Films Using Trimethylaluminum and Ethylene Glycol. Chemistry of Materials 2007, (In Press). 27. Chen, Z.; Cotterell, B.; Wang, W.; Guenther, E.; Chua, S.-J., A mechanical assessment of flexible optoelectronic devices. Thin Solid Films 2001, 394 (1-2), 201-205. 28. Cairns, D. R.; Richard, P. W., II; Daniel, K. S.; Suzanne, M. S.; David, C. P.; Gregory, P. C.; Newton, R. R., Strain-dependent electrical resistance of tin-doped indium oxide on polymer substrates. Applied Physics Letters 2000, 76 (11), 1425-1427. 29. Crawford, G. P., Flexible flat panel displays. John Wiley & Sons, Ltd.: 2005. 30. Leterrier, Y.; Medico, L.; Demarco, F.; Manson, J. A. E.; Betz, U.; Escola, M. F.; Kharrazi Olsson, M.; Atamny, F., Mechanical integrity of transparent conductive oxide films for flexible polymer-based displays. Thin Solid Films 2004, 460 (1-2), 156-166. 31. Paetzold, R.; Heuser, K.; Henseler, D.; Roeger, S.; Wittmann, G.; Winnacker, A., Performance of flexible polymeric light-emitting diodes under bending conditions. Applied Physics Letters 2003, 82 (19), 3342-3344. 32. Dameron, A. A.; Davidson, S. D.; Burton, B. B.; Carcia, P. F.; McLean, R. S.; George, S. M., Gas Diffusion Barriers on Polymers Using Multilayers Fabricated by Al2O3 and Rapid SiO2 Atomic Layer Deposition. The Journal of Physical Chemistry C 2008, 112 (12), 4573-4580. 33. G. Nisato, P. C. P. B., P. J. Slikkerveer, W. D. Bennett, G. L. Graff, N. Rutherford, and L. Wiese, Evaluating high performance diffusion barriers: The calcium test. Proc. Asia Display 2001, 1435-1438. 34. Paetzold, R.; Winnacker, A.; Henseler, D.; Cesari, V.; Heuser, K., Permeation rate measurements by electrical analysis of calcium corrosion. Review of Scientific Instruments 2003, 74 (12), 5147-5150. 35. Kim, T. W.; Yan, M.; Erlat, A. G.; McConnelee, P. A.; Pellow, M.; Deluca, J.; Feist, T. P.; Duggal, A. R.; Schaepkens, M. In Transparent hybrid inorganic/organic barrier coatings for plastic organic light-emitting diode substrates, AVS: 2005; pp 971-977. 36. Carcia, P. F.; McLean, R. S.; Groner, M. D.; Dameron, A. A.; George, S. M., Gas diffusion ultrabarriers on polymer substrates using Al2O3 atomic layer deposition and SiN plasma-enhanced chemical vapor deposition. Journal of Applied Physics 2009, 106 (2), 023533-6. 37. Jin Hwan, C.; Young Min, K.; Young Wook, P.; Jin Woo, H.; Byeong Kwon, J.; In Sun, K.; Hee Nam, H., Evaluation of gas permeation barrier properties using electrical measurements of calcium degradation. Review of Scientific Instruments 2007, 78 (6), 064701. 38. Zhang, Y.; Bertrand, J. A.; Yang, R.; George, S. M.; Lee, Y. C., Electroplating to visualize defects in Al2O3 thin films grown using atomic layer deposition. Thin Solid Films 2009, 517 (11), 3269-3272. 39. Zhang, Y.; Zhang, Y.-Z.; Miller, D. C.; Bertrand, J. A.; Jen, S.-H.; Yang, R.; Dunn, M. L.; George, S. M.; Lee, Y. C., Fluorescent tags to visualize defects in Al2O3 thin films grown using atomic layer deposition. Thin Solid Films 2009, 517 (24), 6794-6797.
![Page 138: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/138.jpg)
126
40. Merlo, G. B. a. F., Crystal Chemical Remarks on the Alloying Behavior of Calcium, Strontium and Barium. Journal of the Less-Common Metals 1982, 85, 285-306. 41. Merlo, F., Crystal Structures of CaAg, CaAu and SrZn. Journal of Less-Common Metals 1982, 86, 241-246. 42. Notin, M.; Mejbar, J.; Bouhajib, A.; Charles, J.; Hertz, J., The Thermodynamic Properties of Calcium Intermetallic Compounds. Journal of Alloys and Compounds 1995, 220 (1-2), 62-75. 43. Miura, H.; Itabashi, I.; Yu, G.; Sakai, T., Grain refinement of coarse grained gold by combined thermo-mechanical process of severe plastic deformation and low temperature annealing. Journal of Physics: Conference Series 2010, 240 (1), 012116. 44. Rocklein, M. N.; George, S. M., Temperature-Induced Apparent Mass Changes Observed during Quartz Crystal Microbalance Measurements of Atomic Layer Deposition. Anal. Chem. 2003, 75 (19), 4975-4982. 45. Elam, J. W.; Groner, M. D.; George, S. M., Viscous flow reactor with quartz crystal microbalance for thin film growth by atomic layer deposition. Review of Scientific Instruments 2002, 73 (8), 2981-2987. 46. Jen, S. B., J. A.; George, S. M., Critical tensile and compressive strains for cracking of Al2O3 films grown by atomic layer deposition. J. Appl. Phys. 2011, 109 (8), 084305. 47. Greenspan, L., Humidity fixed points of binary saturated aqueous solutions. J. Res. Nat. Bur. Stand. A 1977, 81A (1), 8. 48. Lu, T.; Chen, C., Uncertainty evaluation of humidity sensors calibrated by saturated salt solutions. Measurement 2007, 40 (6), 591-599. 49. Hauch, J. A.; Schilinsky, P.; Choulis, S. A.; Rajoelson, S.; Brabec, C. J., The impact of water vapor transmission rate on the lifetime of flexible polymer solar cells. Appl. Phys. Lett. 2008, 93 (10), 103306. 50. Lewis, J. S.; Weaver, M. S., Thin-film permeation-barrier technology for flexible organic light-emitting devices. IEEE J. Sel. Top. Quant. Elect. 2004, 10 (1), 45-57. 51. Nisato, G.; Bouten, P. C. P.; Slikkerveer, P. J.; Bennett, W. D.; Graff, G. L.; Rutherford, N.; Wiese, L., Evaluating Higher Performance Diffusion Barriers: the Calcium Test. Proc. Asia Display/IDW '01 2001, 1435. 52. Ranade, A.; D'Souza, N. A.; Wallace, R. M.; Gnade, B. E., High sensitivity gas permeability measurement system for thin plastic films. Review of Scientific Instruments 2005, 76 (1). 53. Zhang, X. D.; Lewis, J. S.; Wolter, S. D.; Parker, C. B.; Glass, J. T., High sensitivity permeation measurement system for "ultrabarrier" thin films. Journal of Vacuum Science & Technology A 2007, 25 (6), 1587-1593. 54. Dunkel, R.; Bujas, R.; Klein, A.; Horndt, V., Method of measuring ultralow water vapor permeation for OLED displays. Proceedings of the Ieee 2005, 93 (8), 1478-1482. 55. Groner, M. D.; George, S. M.; McLean, R. S.; Carcia, P. F., Gas diffusion barriers on polymers using Al2O3 atomic layer deposition. Appl. Phys. Lett. 2006, 88 (5), 051907. 56. Schubert, S.; Klumbies, H.; Muller-Meskamp, L.; Leo, K., Electrical calcium test for moisture barrier evaluation for organic devices. Review of Scientific Instruments 2011, 82 (9). 57. Carcia, P. F.; McLean, R. S.; Groner, M. D.; Dameron, A. A.; George, S. M., Gas diffusion ultrabarriers on polymer substrates using Al2O3 atomic layer deposition and SiN plasma-enhanced chemical vapor deposition. J. Appl. Phys. 2009, 106 (2), 023533. 58. Kim, T. W.; Yan, M.; Erlat, G.; McConnelee, P. A.; Pellow, M.; Deluca, J.; Feist, T. P.; Duggal, A. R.; Schaepkens, M., Transparent hybrid inorganic/organic barrier coatings for plastic organic light-emitting diode substrates. Journal of Vacuum Science & Technology A 2005, 23 (4), 971-977. 59. Carcia, P. F.; McLean, R. S.; Reilly, M. H.; Groner, M. D.; George, S. M., Ca test of Al2O3 gas diffusion barriers grown by atomic layer deposition on polymers. Appl. Phys. Lett. 2006, 89 (3), 031915.
![Page 139: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/139.jpg)
127
60. Ferrari, S.; Perissinotti, F.; Peron, E.; Fumagalli, L.; Natali, D.; Sampietro, M., Atomic layer deposited Al2O3 as a capping layer for polymer based transistors. Organic Electronics 2007, 8 (4), 407-414. 61. Kim, N.; Potscavage, W. J.; Domercq, B.; Kippelen, B.; Graham, S., A hybrid encapsulation method for organic electronics. Applied Physics Letters 2009, 94 (16). 62. Langereis, E.; Creatore, M.; Heil, S. B. S.; Van de Sanden, M. C. M.; Kessels, W. M. M., Plasma-assisted atomic layer deposition of Al2O3 moisture permeation barriers on polymers. Applied Physics Letters 2006, 89 (8). 63. Meyer, J.; Schneidenbach, D.; Winkler, T.; Hamwi, S.; Weimann, T.; Hinze, P.; Ammermann, S.; Johannes, H. H.; Riedl, T.; Kowalsky, W., Reliable thin film encapsulation for organic light emitting diodes grown by low-temperature atomic layer deposition. Applied Physics Letters 2009, 94 (23). 64. Elam, J. W.; Groner, M. D.; George, S. M., Viscous flow reactor with quartz crystal microbalance for thin film growth by atomic layer deposition. Rev. Sci. Instrum. 2002, 73 (8), 2981-2987. 65. Dillon, A. C.; Ott, A. W.; Way, J. D.; George, S. M., Surface-Chemistry of Al2O3 Deposition Using Al(CH3)3 and H2O in a Binary Reaction Sequence. Surf. Sci. 1995, 322 (1-3), 230-242. 66. Ott, A. W.; Klaus, J. W.; Johnson, J. M.; George, S. M., Al3O3 thin film growth on Si(100) using binary reaction sequence chemistry. Thin Solid Films 1997, 292 (1-2), 135-144. 67. Greenspan, L., Humidity Fixed-Points of Binary Saturated Aqueous-Solutions. Journal of Research of the National Bureau of Standards Section a-Physics and Chemistry 1977, 81 (1), 89-96. 68. Lu, T. H.; Chen, C. C., Uncertainty evaluation of humidity sensors calibrated by saturated salt solutions. Measurement 2007, 40 (6), 591-599. 69. Sobrinho, A. S. D.; Czeremuszkin, G.; Latreche, M.; Wertheimer, M. R., Defect-permeation correlation for ultrathin transparent barrier coatings on polymers. Journal of Vacuum Science & Technology a-Vacuum Surfaces and Films 2000, 18 (1), 149-157. 70. Sobrinho, A. S. D.; Latreche, M.; Czeremuszkin, G.; Klemberg-Sapieha, J. E.; Wertheimer, M. R., Transparent barrier coatings on polyethylene terephthalate by single- and dual-frequency plasma-enhanced chemical vapor deposition. Journal of Vacuum Science & Technology A 1998, 16 (6), 3190-3198. 71. Dameron, A. A.; Davidson, S. D.; Burton, B. B.; Carcia, P. F.; McLean, R. S.; George, S. M., Gas diffusion barriers on polymers using multilayers fabricated by Al2O3 and rapid SiO2 atomic layer deposition. Journal of Physical Chemistry C 2008, 112 (12), 4573-4580. 72. Iftekhar, S.; Grins, J.; Svensson, G.; Loof, J.; Jarmar, T.; Botton, G. A.; Andrei, C. M.; Engqvist, H., Phase formation of CaAl2O4 from CaCO3-Al2O3 powder mixtures. J. Eur. Ceram. Soc. 2008, 28 (4), 747-756. 73. Lind, M.; Holappa, L., Transformation of Alumina Inclusions by Calcium Treatment. Metall. Mater. Trans. B 2010, 41 (2), 359-366. 74. Granstrom, J.; Villet, M.; Chatterjee, T.; Gerbec, J. A.; Jerkunica, E.; Roy, A., Multilayer barrier films comprising nitrogen spacers between free-standing barrier layers. Applied Physics Letters 2009, 95 (9). 75. Choi, J. H.; Kim, Y. M.; Park, Y. W.; Huh, J. W.; Ju, B. K.; Kim, I. S.; Hwang, H. N., Evaluation of gas permeation barrier properties using electrical measurements of calcium degradation. Review of Scientific Instruments 2007, 78 (6). 76. Reese, M. O.; Dameron, A. A.; Kempe, M. D., Quantitative calcium resistivity based method for accurate and scalable water vapor transmission rate measurement. Review of Scientific Instruments 2011, 82 (8). 77. Chen, T. N.; Wuu, D. S.; Wu, C. C.; Chiang, C. C.; Chen, Y. P.; Horng, R. H., Improvements of permeation barrier coatings using encapsulated parylene interlayers for flexible electronic applications. Plasma Processes and Polymers 2007, 4 (2), 180-185.
![Page 140: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/140.jpg)
128
78. Saitoh, K.; Kumar, R. S.; Chua, S.; Masuda, A.; Matsumura, H., Estimation of moisture barrier ability of thin SiNx single layer on polymer substrates prepared by Cat-CVD method. Thin Solid Films 2008, 516 (5), 607-610. 79. Sobrinho, A. S. D.; Czeremuszkin, G.; Latreche, M.; Dennler, G.; Wertheimer, M. R., A study of defects in ultra-thin transparent coatings on polymers. Surface & Coatings Technology 1999, 116, 1204-1210. 80. Zhang, Y. D.; Bertrand, J. A.; Yang, R. G.; George, S. M.; Lee, Y. C., Electroplating to visualize defects in Al2O3 thin films grown using atomic layer deposition. Thin Solid Films 2009, 517 (11), 3269-3272. 81. Zhang, Y. D.; Zhang, Y. Z.; Miller, D. C.; Bertrand, J. A.; Jen, S. H.; Yang, R. G.; Dunn, M. L.; George, S. M.; Lee, Y. C., Fluorescent tags to visualize defects in Al2O3 thin films grown using atomic layer deposition. Thin Solid Films 2009, 517 (24), 6794-6797. 82. Carcia, P. F.; McLean, R. S.; Reilly, M. H., Permeation measurements and modeling of highly defective Al2O3 thin films grown by atomic layer deposition on polymers. Applied Physics Letters 2010, 97 (22). 83. Stathis, J. H., Percolation models for gate oxide breakdown. Journal of Applied Physics 1999, 86 (10), 5757-5766. 84. Sune, J., New physics-based analytic approach to the thin-oxide breakdown statistics. Ieee Electron Device Letters 2001, 22 (6), 296-298. 85. Nahar, R. K., Study of the performance degradation of thin film aluminum oxide sensor at high humidity. Sensors and Actuators B-Chemical 2000, 63 (1-2), 49-54. 86. Nahar, R. K., Physical understanding of moisture induced degradation of nanoporous aluminum oxide thin films. Journal of Vacuum Science & Technology B 2002, 20 (1), 382-385. 87. Ghosh, A. P.; Gerenser, L. J.; Jarman, C. M.; Fornalik, J. E., Thin-film encapsulation of organic light-emitting devices. Applied Physics Letters 2005, 86 (22). 88. Abdulagatov, A. I.; Yan, Y.; Cooper, J. R.; Zhang, Y.; Gibbs, Z. M.; Cavanagh, A. S.; Yang, R. G.; Lee, Y. C.; George, S. M., Al2O3 and TiO2 Atomic Layer Deposition on Copper for Water Corrosion Resistance. Acs Applied Materials & Interfaces 2011, 3 (12), 4593-4601. 89. de Csernatony, L., The properties of Viton "A" elastomers--III. Steady state and transient activated gas emission processes from Viton "A" Microelectronics Reliability 1967, 16 (5), 247-251. 90. Dennler, G.; Lungenschmied, C.; Neugebauer, H.; Sariciftci, N. S.; Latrèche, M.; Czeremuszkin, G.; Wertheimer, M. R., A new encapsulation solution for flexible organic solar cells. Thin Solid Films 2006, 511–512 (0), 349-353. 91. Reese, M. O.; Dameron, A. A.; Kempe, M. D., Quantitative calcium resistivity based method for accurate and scalable water vapor transmission rate measurement. Review of Scientific Instruments 2011, 82 (8), 085101-10. 92. Brown, D. E.; George, S. M.; Huang, C.; Wong, E. K. L.; Rider, K. B.; Smith, R. S.; Kay, B. D., H2O Condensation Coefficient and Refractive Index for Vapor-Deposited Ice from Molecular Beam and Optical Interference Measurements. The Journal of Physical Chemistry 1996, 100 (12), 4988-4995. 93. Wang, Z. F.; Wang, B.; Ding, X. M.; Zhang, M.; Liu, L. M.; Qi, N.; Hu, J. L., Effect of temperature and structure on the free volume and water vapor permeability in hydrophilic polyurethanes. Journal of Membrane Science 2004, 241 (2), 355-361. 94. Wang, Z. F.; Wang, B.; Qi, N.; Ding, X. M.; Hu, J. L., Free volume and water vapor permeability properties in polyurethane membranes studied by positrons. Materials Chemistry and Physics 2004, 88 (1), 212-216. 95. Morisato, A.; Pinnau, I., Synthesis and gas permeation properties of poly(4-methyl-2-pentyne). Journal of Membrane Science 1996, 121 (2), 243-250.
![Page 141: Gas Diffusion Barriers Using Atomic Layer Deposition: A](https://reader030.vdocuments.mx/reader030/viewer/2022012619/61a06ac3ecf3374a935b505c/html5/thumbnails/141.jpg)
129
96. Kim, H.; Horwitz, J. S.; Kim, W. H.; Makinen, A. J.; Kafafi, Z. H.; Chrisey, D. B., Doped ZnO thin films as anode materials for organic light-emitting diodes. Thin Solid Films 2002, 420-421, 539-543. 97. Lee, S. T.; Gao, Z. Q.; Hung, L. S., Metal diffusion from electrodes in organic light-emitting diodes. Applied Physics Letters 1999, 75 (10), 1404-1406. 98. Tadatsugu, M., Transparent conducting oxide semiconductors for transparent electrodes. Semiconductor Science and Technology 2005, (4), S35. 99. Elam, J. W.; Routkevitch, D.; George, S. M., Properties of ZnO/Al2O3 Alloy Films Grown Using Atomic Layer Deposition Techniques. Journal of The Electrochemical Society 2003, 150 (6), G339-G347. 100. Ellmer, K., Resistivity of polycrystalline zinc oxide films: current status and physical limit. Journal of Physics D: Applied Physics 2001, 34 (21), 3097-3108. 101. Cordero, N.; Yoon, J.; Suo, Z., Channel cracks in a hermetic coating consisting of organic and inorganic layers. Applied Physics Letters 2007, 90 (11), 111910-3. 102. Andersons, J.; Modniks, J.; Leterrier, Y.; Tornare, G.; Dumont, P.; Månson, J. A. E., Evaluation of toughness by finite fracture mechanics from crack onset strain of brittle coatings on polymers. Theoretical and Applied Fracture Mechanics 2008, 49 (2), 151-157.