en-gjs-500-14 properties
DESCRIPTION
This is a snapshot of the chemical and physical properties of EN-GJS-500-14 SG Iron CastingsTRANSCRIPT
Grade : EN-GJS-500-14
Number: 5.3109
Standard: EN 1563 : 2011 Founding. Spheroidal graphite cast irons
Density: 7 g/cm ³
Classification: Spheroidal graphite cast iron
Equivalent grades: No information
Chemical composition % of grade EN-GJS-500-14 (5.3109)
Si content may be lower due to other alloying elements With lower Mn content (e.g. 0.3%), machinability and elongation will be improved
Si Mn P
max 3.8 max 0.5 max 0.05
Mechanical properties of grade EN-GJS-500-14 (5.3109)
Nominal thickness (mm): to 30 30 - 60
Rm - Tensile strength (MPa) 500 480
Nominal thickness(mm): to 30 30 - 60
Rp0.2 0.2% proof strength (MPa) 400 390
Nominal thickness (mm): to 30 30 - 60
A - Min. elongation at fracture (%) 14 12
Brinell hardness (HBW): 170 - 215