creep testing on plastics and composites · tb. strain results determined beyond a yield point are...

21
Intelligent testing Lukas Unger June 18, 2019 Creep testing on plastics and composites

Upload: others

Post on 03-Aug-2020

8 views

Category:

Documents


1 download

TRANSCRIPT

Page 1: Creep testing on plastics and composites · tB. Strain results determined beyond a yield point are measured as ... Creep testing on plastics and composites Material Meets Engineering

Intelligent testing

Lukas Unger

June 18, 2019

Creep testingon plastics and composites

Page 2: Creep testing on plastics and composites · tB. Strain results determined beyond a yield point are measured as ... Creep testing on plastics and composites Material Meets Engineering

Creep testing on plastics and compositesMaterial Meets Engineering 2019

June 18, 2019Lukas Unger

Agenda

2

Working principles plastics / composites

Characteristics of creep testing systems

Standards / Requirements

Page 3: Creep testing on plastics and composites · tB. Strain results determined beyond a yield point are measured as ... Creep testing on plastics and composites Material Meets Engineering

Creep testing on plastics and compositesMaterial Meets Engineering 2019

June 18, 2019Lukas Unger

Tensile tests Creep testson plastics

Strain modeling

RelaxationTests

Steppedisothermal

method (SIM)

Full Notch Creep Test

(FNCT)

Creep tests on composites

ISO 527 ISO 899 R&D ISO 3384-1 R&D ISO 16770 ASTM D7337

Common test types - Overview

3

Applications

t

…σ

t

T

t

σ

t

T

t

σ

σ1

σ2

t

T

t

ε …

t

T

t

…σ

t

T

t

T

t

T

ε

σ

t

…σ

Page 4: Creep testing on plastics and composites · tB. Strain results determined beyond a yield point are measured as ... Creep testing on plastics and composites Material Meets Engineering

Creep testing on plastics and compositesMaterial Meets Engineering 2019

June 18, 2019Lukas Unger

Tensile test

4

Applications

ab

c

d

Stress-strain curve types:

Curve a: Brittle materials

Curve b and c: Tough materials with yield point

Curve d: Tough materials without yield point

Results:

Tensile-Modulus, Et

Yield (εy, σy)

maximum force , σM, εM,

Break point, σB, εB, εtB

Strain results determined beyond a yield point are measured as “Nominal Strain”

HT tensile tests

ISO 527

t

T

ε

σ

Source: ISO 527-1

Page 5: Creep testing on plastics and composites · tB. Strain results determined beyond a yield point are measured as ... Creep testing on plastics and composites Material Meets Engineering

Creep testing on plastics and compositesMaterial Meets Engineering 2019

June 18, 2019Lukas Unger

Creep test on plastics

5

Applications

Requirements: Test duration

Usually 1.000h

Load (stress) control: Class 1

Wide measure range

Temperature

Accuracy: ± 2K

Wide Temperature Range

No overshooting

Reliable System:

Data Safety Concept

Strain Measurement: Class 1

Class 1 and Class 0.5

Creep tests

ISO 899-1, -2ASTM D2990

t

σ

t

T

Results: Initial plastic strain

Creep strain

Time to specific creep strain

Creep strength (time to fracture acc. to stress level)

Creep limits (time to strain limit acc. to stress level)

Creep modulus (stress to strain versus time)

PRIMARY

SECONDARY

TERTIARY

TOTA

L ST

RAI

N

TIME

INITIAL PLASTIC STRAIN

INITIAL ELASTIC STRAIN

FRACTURE

Source: ASTM D2990

Page 6: Creep testing on plastics and composites · tB. Strain results determined beyond a yield point are measured as ... Creep testing on plastics and composites Material Meets Engineering

Creep testing on plastics and compositesMaterial Meets Engineering 2019

June 18, 2019Lukas Unger

The Stepped Isothermal Method (SIM) offers savings of time and costsby temperature steps on 1 specimen.

6

Applications

Tem

pera

ture

(°C

)

Time (s)

Temperature steps

Source: SKZ (http://www.skz.de)

Steppedisothermal

method (SIM)

R&D

t

…σ

t

T

Page 7: Creep testing on plastics and composites · tB. Strain results determined beyond a yield point are measured as ... Creep testing on plastics and composites Material Meets Engineering

Creep testing on plastics and compositesMaterial Meets Engineering 2019

June 18, 2019Lukas Unger

With temperature steps the creep strain is increasing.

7

Applications

Tem

pera

ture

(°C

)

Time (s)

Temperature steps

Stra

in (%

)

Source: SKZ (http://www.skz.de)

Steppedisothermal

method (SIM)

R&D

t

…σ

t

T

Page 8: Creep testing on plastics and composites · tB. Strain results determined beyond a yield point are measured as ... Creep testing on plastics and composites Material Meets Engineering

Creep testing on plastics and compositesMaterial Meets Engineering 2019

June 18, 2019Lukas Unger

According to SIM the steps are handled as separate virtual creep tests.

8

ApplicationsTe

mpe

ratu

re (°

C)

Time (s)

Temperature steps

Stra

in (%

)Source: SKZ (http://www.skz.de)

Stra

in (%

)

Page 9: Creep testing on plastics and composites · tB. Strain results determined beyond a yield point are measured as ... Creep testing on plastics and composites Material Meets Engineering

Creep testing on plastics and compositesMaterial Meets Engineering 2019

June 18, 2019Lukas Unger

With SIM the separate creep strain curves are combined to a master curve.

9

Applications

Source: SKZ (http://www.skz.de)

Stra

in (%

)

Stra

in (%

)

Stra

in (%

)

Log (Time) at T0 after displacement

logarithmicscale Master curve at T0

Page 10: Creep testing on plastics and composites · tB. Strain results determined beyond a yield point are measured as ... Creep testing on plastics and composites Material Meets Engineering

Creep testing on plastics and compositesMaterial Meets Engineering 2019

June 18, 2019Lukas Unger

Agenda

10

Working principles plastics / composites

Characteristics of Creep Testing Systems

Standards / Requirements

Page 11: Creep testing on plastics and composites · tB. Strain results determined beyond a yield point are measured as ... Creep testing on plastics and composites Material Meets Engineering

Creep testing on plastics and compositesMaterial Meets Engineering 2019

June 18, 2019Lukas Unger

HT tensile tests

Creep testson plastics

(up to 10 kN)

Strain modeling

RelaxationTests

Steppedisothermal

method(SIM)

Full Notch Creep Test

(FNCT)

Creep tests on composites(up to 50 kN)

t

σ

t

σ

σ1

σ2

t

…σ

ε

σ

Electromechanical Multistation Creep testers offer most flexible range of applications.

Multistation LA Multistation 5 x 10kN Multistation 3 x 50kN

11

Direct weight

t

ε …

Working principles – plastics and composites

t

…σ

t

σ

Page 12: Creep testing on plastics and composites · tB. Strain results determined beyond a yield point are measured as ... Creep testing on plastics and composites Material Meets Engineering

Creep testing on plastics and compositesMaterial Meets Engineering 2019

June 18, 2019Lukas Unger

12

The electromechanical Kappa Multistation can be used for flexible loads and flexible applications.

Working principles – plastics and composites

Characteristics Load range: 20N – 10.000N

Application range: tensile, flexure, compressionload (stress) control, strain control

5 to 6 test axes per load frame

Central spindle with each test axis and individual closed-loop-control

One temperature chamber for all test axes

Alternatively two temperature chambers in one load frame (each for maximum 3 test axes)

Non-contacting strain measurement(recommended by testing standards)

Page 13: Creep testing on plastics and composites · tB. Strain results determined beyond a yield point are measured as ... Creep testing on plastics and composites Material Meets Engineering

Creep testing on plastics and compositesMaterial Meets Engineering 2019

June 18, 2019Lukas Unger

13

Strain measurement

13

Non-contacting videoXtens for strain measurement withaccuracy class 1 without any influence on the specimen.

Rear view

Non-contacting video-extensometer

1 videoXtens system

1 camera for each test axes

Strain measurement accuracy class 1(class 0.5 on request)

Quick set up for testing

No influence (notching) on specimen

Stable temperature (view through glass window)

Flexible gauge length and measurement range

Range of application: Tensile, Flexure, compression

Front view

Page 14: Creep testing on plastics and composites · tB. Strain results determined beyond a yield point are measured as ... Creep testing on plastics and composites Material Meets Engineering

Creep testing on plastics and compositesMaterial Meets Engineering 2019

June 18, 2019Lukas Unger

14

Test types

14

Non-contacting videoXtens for strain and deformation measurement on different applications.

Setup for creep tensile Setup for creep compression Setup for creep flexure

Page 15: Creep testing on plastics and composites · tB. Strain results determined beyond a yield point are measured as ... Creep testing on plastics and composites Material Meets Engineering

Creep testing on plastics and compositesMaterial Meets Engineering 2019

June 18, 2019Lukas Unger

Agenda

15

Working principles plastics / composites

Characteristics of Creep Testing Systems

Standards / Requirements

Page 16: Creep testing on plastics and composites · tB. Strain results determined beyond a yield point are measured as ... Creep testing on plastics and composites Material Meets Engineering

Creep testing on plastics and compositesMaterial Meets Engineering 2019

June 18, 2019Lukas Unger

16

Kappa Multistation

16

The basic system features 5 or 6 testing axis incl. temperature chamber.

Individually controlled test axes

Each test axis equipped with 1 fix mounted camera

Temperature range: (LN2: - 30°C) … 35°C … + 250°C

Page 17: Creep testing on plastics and composites · tB. Strain results determined beyond a yield point are measured as ... Creep testing on plastics and composites Material Meets Engineering

Creep testing on plastics and compositesMaterial Meets Engineering 2019

June 18, 2019Lukas Unger

17

Types of tests

17

Different applications can be operated in 1 testing system.

Setup for creep-tensile Setup for creep-3-point flexure

Setup for creep-4-point flexure

Setup for compression

Page 18: Creep testing on plastics and composites · tB. Strain results determined beyond a yield point are measured as ... Creep testing on plastics and composites Material Meets Engineering

Creep testing on plastics and compositesMaterial Meets Engineering 2019

June 18, 2019Lukas Unger

Temperature chamber “Fridge-type”

18

Kappa Multistation with fridge-type temperature chamber is used for long term test at sub-zero temperatures.

Temperature range: - 10°C … + 100°C

Page 19: Creep testing on plastics and composites · tB. Strain results determined beyond a yield point are measured as ... Creep testing on plastics and composites Material Meets Engineering

Creep testing on plastics and compositesMaterial Meets Engineering 2019

June 18, 2019Lukas Unger

Creep tests on plastics in controlled humidity environment from +20°C to 90°C – without humidity control -30°C up to +180°C.

Temperature + Climatic Chamber

28

Page 20: Creep testing on plastics and composites · tB. Strain results determined beyond a yield point are measured as ... Creep testing on plastics and composites Material Meets Engineering

Creep testing on plastics and compositesMaterial Meets Engineering 2019

June 18, 2019Lukas Unger

Fiber Reinforced Polymer Matrix Composite Bars

20

Testing plastics and composites according to ISO 899-1 and ASTM D7337 up to 50 kN per load line at elevated temperatures.

Non-Contact strain measurement: No influence on specimen No damage on extensometer

Load range: 100N … 50.000N

Page 21: Creep testing on plastics and composites · tB. Strain results determined beyond a yield point are measured as ... Creep testing on plastics and composites Material Meets Engineering

Creep testing on plastics and compositesMaterial Meets Engineering 2019

June 18, 2019Lukas Unger

Fiber Reinforced Polymer Matrix Composite Bars

21

Ambient temperature creep tensile test at 20 MPa and a test duration of 100 hours.