andreas brandl - cementing strategies for effective zonal ... · 1st combined network meeting on...
TRANSCRIPT
![Page 1: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/1.jpg)
1st Combined Network Meeting on Modelling and
Wellbore Integrity, Perth Australia, April 27-29, 2 011
Cementing Strategies for Effective Zonal Isolation of CO 2 Wells
Andreas Brandl (Baker Hughes)Scott Bray (Baker Hughes)
Christina Magelky (Baker Hughes) Ragheb Dajani (Hess Corporation)
![Page 2: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/2.jpg)
OVERVIEW
• Review: Zonal Isolation of CO2 wells (field studies)
What can we do ‘in addition’ to prevent leakage?
• Sealing Spacer improves cement placement
• Expanding cement system supporting bond
• CO2 tolerable cement for long term bond
![Page 3: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/3.jpg)
RESULTS FROM FIELD STUDIES
• Portland cement degradation due to CO2: <10 mm / 30 yrs (J.W. Carey et al. 2007)
• Degradation mainly occurs along existing / induced pathways (B. Kutchko et al. 2009)
• Pozz/Portland cement inhibit CO2 migration after carbonation (W. Crow et al. 2009)
⇒ Leakage only due to CO2 attack very unlikely
⇒ Cements ability to resist CO2 attack is secondary
⇒ Important: Good initial cement bond
![Page 4: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/4.jpg)
OVERVIEW
• Review: Zonal Isolation of CO2 wells (field studies)
What can we do ‘in addition’ to prevent leakage?
1. Sealing Spacer improves cement placement
2. Expanding cement system supporting bond
3. CO2 tolerable cement for long term bond
![Page 5: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/5.jpg)
SEALING SPACER - PURPOSE
Reducing lost circulation problems & damages
• Permeable, fragile, and weak formations
• (Natural) fractures
• Depleted reservoirs
Strengthening wellbore & Allowing cement placement
• Low frac gradients
• Narrow ECD margins (limit cement density)
![Page 6: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/6.jpg)
SEALING SPACER - BENEFITS
Sealing
Typical Spacer
applied prior cementing
Sealing Spacer
applied prior cementing
• Prevents formation breakdown & fall back of cement tops• Strengthens wellbore for improved cement slurry placement
![Page 7: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/7.jpg)
STRENGTHENING OF WELLBORE
Before Sealing Spacer was applied:• Cementing required a stage tool, since desired height exceeded max. ECD of 10.93 ppg
After using Sealing Spacer:• Cementing in single stage at ECD 12.26 ppg• No losses, top of cement found at desired top
=> Operator saved time & money with a high quality cement job
![Page 8: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/8.jpg)
SEALING SPACER’s EFFICIENCY
Sealing Spacer
Typical Spacer
No flow
Blow
out
No losses when Sealing Spacer is applied
20/40
frac sand
![Page 9: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/9.jpg)
MORE BENEFITS OF THE SEALING
CO2
Mg2+
H2S
Sealing
SO42-
• Sealing acts like a “condom”• Potentially protects cement sheath towards corrosive fluids
![Page 10: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/10.jpg)
OVERVIEW
• Review: Zonal Isolation of CO2 wells (field studies)
What can we do ‘in addition’ to prevent leakage?
1. Sealing Spacer improves cement placement
2. Expanding cement system supporting bond
3. CO2 tolerable cement for long term bond
![Page 11: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/11.jpg)
Expansion and Shrinkage Under Temperature and Pressure
• Patented BHI Molds (US 6,918,292)• Placed in a modified HTHP curing chamber • Measures shrinkage & expansion real time• SPE/IADC 79911
![Page 12: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/12.jpg)
Cement Additives for ExpansionLeft Sample: Class G cement + 0.75% EC-2 + 35% S-8 + 0.8% FL-25 + 0.6% CD-32 + 0.5% R-
8 mixed at 16.7 ppg, Yield = 1.40 cu ft/sk, and Fre sh water = 5.06 gal/sk
-0.3
-0.25
-0.2
-0.15
-0.1
-0.05
0
0.05
0.1
0.15
0 20 40 60 80 100 120 140 160Elapsed Time (hr)
% L
ine
ar
Exp
ans
ion
or S
hrin
kage
0
500
1000
1500
2000
2500
3000
3500
4000
4500
5000
Te
st T
em
pera
ture
(°F
) a
nd P
ress
ure
(ps
i)
Test Temperature
Test Pressure
% linear Expansion
Base-Line
The Cement was heated in 4:00 hrs to its final (BHST) Temperature and Pressure. After 4 hrs, the temp and pres has estabil ized. Any test data above the base-line are consider expansion and below are shrinkage.
Right Sample: Class G cement + 35% S-8 + 5.0% EC-2 + 0.8% FL-25 + 0.6% CD-32 + 0.5% R-8 mixed at 16.7 ppg, Yield = 1.40 cu ft/sk and fres h water = 5.02 gal/sk
-2
0
2
4
6
8
10
12
0 5 10 15 20 25 30 35 40 45 50
Elapsed Time (hr)
% L
ine
ar
Exp
ans
ion
or S
hrin
kage
0
500
1000
1500
2000
2500
3000
3500
4000
Te
st P
ress
ure
(psi
) a
nd T
em
pera
ture
(°F)
% Linear Expansion
Test Temperature
Test Pressure
Out of ranges (expansion device)
Base-line
The cement was heated in 4 hrs to its final (BHST) temperature and pressure. After 4 hrs, the temp and pres has estabil ized. Any test data above the base-line are consider expansion and below are shrinkage.
Delayed hydration of MgO
+ Expansion after cement set
- Overdosage → cracking
![Page 13: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/13.jpg)
Cement Additives for Expansion
Metallic aluminum powder as gas generator
- produces H2 gas in alkaline environment
- difficult to control
- gas generation occurs prior cement setting
Metallic aluminum powder as gas generator
- produces H2 gas in alkaline environment (safety issue)
- difficult to control expansion
- gas generation occurs prior cement setting
![Page 14: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/14.jpg)
Expanding Cement System
+ 13.3 – 15.8 ppg
+ HT polymeric extender
+ Stable @ 465 F
+ No gas generation
+ No shrinkage
+ Controlled Expansion
→ Supports bond
→ Reduces micro annuli
→ Field proven technology (SPE ATC 147012)
![Page 15: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/15.jpg)
OVERVIEW
• Review: Zonal Isolation of CO2 wells (field studies)
What can we do ‘in addition’ to prevent leakage?
1. Sealing Spacer improves cement placement
2. Expanding cement system supporting bond
3. CO2 tolerable cement for long term bond
![Page 16: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/16.jpg)
CO2 Attack in API Cement
I. unaltered set cement
III. carbonated cement
IV. porous silica (soft)
CO2 +
H2O ⇌⇌⇌⇌
H2CO3 ⇌⇌⇌⇌
H+ +
HCO3-
V. corrosive fluid
Leaching frontCarbonation front
C-S-H phases
Ca(OH)2
dissolve
Ca2+aq
OH-aq
precipitates dissolves
Ca2+aq
H+aq
HCO3-aq
CaCO3
SPE 132228-PA
![Page 17: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/17.jpg)
After 6 Months Exposure to CO 2
Cement specimen flaked off (diameter ∆=-0.6 mm)Cement bond failure / migration pathways => Loss of zonal isolation
CO2 tolerable cement Conventional
![Page 18: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/18.jpg)
Exposed to 1 M HCl (24 hrs)
2 H+ + Ca(OH)2 Ca2+ + 2 H2O
12 H+ + C6-S5-H6 6 Ca2+ + 5 SiO2 + 6 H2O
CO2 tolerable cement Conventional
Simulate: final of leaching step during CO2 exposure
![Page 19: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/19.jpg)
-60%
-50%
-40%
-30%
-20%
-10%
0%
0 50 100 150 200 250 300
Exposure time to 1 molar hydrochloric acid (days)
Loss
of m
ass
(wt%
)
pozzolan
conventional
Durability in 1 M HCl (250 d)
Conventional
CO2 tolerable cement
![Page 20: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/20.jpg)
After 250 d Exposure to 1 M HCl
EDS analyses confirm complete Ca leaching for both
ConventionalCO2 tolerable cement
![Page 21: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/21.jpg)
Conventional
C.S.= 1,520 psiW.P.= 0.00123 mD
• fell apart• no strength• squishy morph.
Durability in 1 M HCl (250 d)
CO2 tolerable cement
![Page 22: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/22.jpg)
Long Term Zonal Isolation0. Seal & Strengthen Formation
1. Follow good practices with API cement based systems (reliable, field proven & practical)
2. Improved cement bonding
3. Design a cement system:• with suitable mechanical properties • preventing strength retrogression• mitigating all corrosive attacks (Mg2+, SO4
2-, H2S, CO2 …)
∆P
∆T
CO2
![Page 23: Andreas Brandl - Cementing Strategies for Effective Zonal ... · 1st Combined Network Meeting on Modelling and Wellbore Integrity, Perth Australia, April 27-29, 2011 Cementing Strategies](https://reader030.vdocuments.mx/reader030/viewer/2022013014/5adbbc797f8b9a53618e5333/html5/thumbnails/23.jpg)
Thank You for Your Interest
PERTH, AUSTRALIA